Rich and others,
Some more history: Short chain silicones would also creep across a PCB and
get into mechanical switches and in the little spark that formed just as the
switch was closing the silicone molecules would decompose to form silica,
another really good insulator that would NOT get out of the way.
Bev
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Richard Kraszewski
Sent: Saturday, August 10, 2013 2:07 PM
To: [log in to unmask]
Subject: Re: [TN] Silicone adhesives on tapes
I only have seen some "suspected" occurrence of this.
Somewhat dependant on how much is deposited, was the tape baked, and if you
have an aromatic solvent based coating. The latter can extract some adhesive
from the tape perimeter.
You can however use Si based tape and never have issues.
I personally think that is tendency to over react to the term silicone.
That is due to hand-soldering where we all learn that silicone hand lotions
hamper solderability (which they can), and older Si Ccings that use some
rather obsolete cure catalyst mechanisms.
Rich Kraszewski
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: Tuesday, August 06, 2013 8:18 AM
To: [log in to unmask]
Subject: [TN] Silicone adhesives on tapes
Do you think the silicone adhesive on Kapton and Shercon tapes can create a
manufacturing issue during conformal coating or for sensitive electronics?
Doug, I would be especially interested in your respected input on this
question.
This message and/or attachments may include information subject to GDC4S
S.P. 1.8.6 and GD Corporate Policy 07-105 and are intended to be accessed
only by authorized recipients. Use, storage and transmission are governed by
General Dynamics and its policies. Contractual restrictions apply to third
parties. Recipients should refer to the policies or contract to determine
proper handling. Unauthorized review, use, disclosure or distribution is
prohibited. If you are not an intended recipient, please contact the sender
and destroy all copies of the original message.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|
|
|