Hi Guy - yes, that is a false idea. The root cause of land lifting with
SnBi solder alloys and shrinkage cracks for most lead-free solder alloys
is simple solidification behavior. One of the reasons that SnPb solder
alloys were selected for use as an attachment material for electronics is
that Sn and Pb have an advantageous lower temperature eutectic point in
its phase diagram. A eutectic alloy is a combination of metallic elements
that change from a liquid phase to a solid phase at a specific temperature
without having a "liquid plus solid" region which many folks call the
"mushy zone". Using a eutectic solder alloy such as Sn60 or Sn63 is great
for manufacturing as the solder goes from liquid to solid (like flipping a
light switch) making processing predictable. Shrinkage voids in solder are
the same phenomenon as shrinkage voids in metal casting operations - the
molten metal cools from a liquid to a liquid plus solid then to a solid.
Since most metals become more dense (aka shrink), the last regions of
molten metal that solidify leaving empty space = shrinkage cracks or
fissures. One of the reasons that the 96.5Sn/3.5Ag solder alloy is also
widely used is that it is a eutectic alloy with a melting point of 221C.
Think of eutectic solder alloys a metal alloys that solidify instantly in
contrast to many other solder alloys with have to do the whole
solidification process.
Dave
From: "Guy Ramsey" <[log in to unmask]>
To: "'TechNet E-Mail Forum'" <[log in to unmask]>,
<[log in to unmask]>
Date: 07/22/2013 06:14 AM
Subject: RE: [TN] NTC Friday Element Quiz Answer
Interesting. I thought that the land lift phenomenon was due to the fact
that SnBi solder shrinks on solidification. And that SnPb solder expands.
Is this false?
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Friday, July 19, 2013 8:17 PM
To: [log in to unmask]
Subject: [TN] NTC Friday Element Quiz Answer
Hi folks - Here is the Friday Element Quiz Answer:
The Question:
This element has some strange properties. The element will melt in your
hand due to body heat and it expands when changing from a liquid to a
solid. It is associated with the town of Gran Sasso, Italy. What element
is being described?
The Answer:
The element is Gallium (Ga)! Gallium is one of three metals that expands
upon solidification (kudos to Ian Fox for knowing that clue) and its
melting point is low enough that human body heat can melt it. Both the
Italian National Lab at Gran Sasso and SAGE lab in Russia use gallium for
their neutrino research. The facility at Gran Sasso has a "tank" of
250,000 pounds of gallium trichloride (GaCl3)! When a neutrino passes thru
the tank, the GaCl3 is converted into germanium 71 isotope which is
detectable by instrumentation (kudos to Mike Fenner for getting that
clue). Neutrinos are particles from the sun that bombard the Earth and can
pass thru miles of solid rock.
The winner of the weekly element quiz is Phil Kinner and he will get the
services of Clumpy and Kloumpios for the week. Lots of good answers this
week and apparently some electronic near misses (Sorry Mike). The boys
caught a cargo flight and are heading to work for Phil for the week.
So far Clumpy and Kloumpios have done the following:
Past Quiz winners/tasks:
Week 1 Dick Krug, Spartan Complex Systems
Week 2 Laura Turbini, IRC
Week 3 James Head, Crowcon Detection Instruments Limited
Week 3 Pat Goodyear, PGE
Week 4 Joe Russeau, Precision Analysts Laboratory
Week 5 Tom Carroll, Boeing Defense, Space and Security
Week 6 Steve Gregory
Week 7 Phil Kinner
Week 8 Brian Ellis
Week 9 James Head, Crowcon Detection Instruments Limited
Week 10 Leland Woodall, CSTech Inc.
Week 11 Keith Calhoun, Sopark Corp
Week 12 Matthias Mansfeld, Mansfeld-Elektronik
Week 13 Leland Woodall, CSTech Inc.
Week 14 Brian Ellis
Week 15 Tom Carroll, Boeing Defense, Space and Security
Week 16 Steve Gregory
Week 17 Phil Kinner
Week 18 Ian Braddock, MBDA Systems
Week 19 Leland Woodall, CSTech Inc.
- Now I have two guys to assist with four screen printer moves this week.
They're gonna love helping me perform our quality verifications, and they
get to try their hand with cross section work again.
Week 20 Denny Fritz
- My first thought for Clumpy and Kloumpios was to ask if they knew how to
drain swamps. It has rained here in Indiana almost every day for 10 days
and is forecast to thunderstorm for almost ten more. Any chance Kloumpios
has any biblical roots and is related to Noah of Ark fame?? At the very
least, please have Graham Naisbitt ship some wellies (Wellington boots)
here to Indiana for the coming week. Only slightly more seriously, what do
Clumpy and Kloumpios know about counterfeit components? Any day, I expect
to be thrown into that messy topic to support the Department of Defense.
And, what clearance do the guys have - confidential, secret, top secret,
or keep-from-telling-Doug?. Can either run an XRF or SEM? I presume they
have eagle eyes, so they can observe components through our optical
microscopes. Finally, is either carrying a small spare lead-acid battery?
Our UPS unit protecting the instruments from the too frequent lightning
surges crapped out last week.
Week 21 Amol Kane
- the boys can help me with optimization and qualification of Process
Equipment like stencil printer and wash. In their spare time they can
enjoy the fine TX summer
Dewey Whittaker, Honeywell
- the boys can stay 2 days with me and as I've always said "a man's home
is his castle, in a manor of speaking". I'll be training them in stand-up
comedy dealing with the dichotomy of Technet humor. Their names and act
will be " Grim and Stellar".
David Bealer, Watch Fire Signs
- since I will be out next week, they can take those 2 days
off. Everybody deserves a weekend once in a while.
Week 22 Phil Kinner
- assisted with ?
Everyone have a safe week!
Dave Hillman
Rockwell Collins
[log in to unmask]
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|