TECHNET Archives

June 2013

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Thu, 6 Jun 2013 16:19:24 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
MIME-Version:
1.0
Message-ID:
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="us-ascii"
From:
Gerald Bogert <[log in to unmask]>
Parts/Attachments:
text/plain (30 lines)
June 6, 2013

 

We have an OM who soldered surface mount Opto-couplers with Sn98/Bi2.5
leads using Sn63Pb37 solder.  The reflow solder profile used was the
traditional one for Sn63 solder with a measured peak temperature in the
range of 209 to 215C.  The actual amount of Bi by weight that wound up
in the completed solder joint was calculated to be about 0.19%.  Based
on this, there is no issue with a low temperature alloy forming with the
combination of Bi and Pb.  

 

However, since the melting point of the Sn98/Bi2.5 solder is around
223-231C, the reflow profile used will not result in melting of the
solder on the part terminations.  Is this an issue or will the Sn63
properly bond to the solder on the part terminations to form an
acceptable solder joint?

 

[log in to unmask]


______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2