At the locations were you are seeing bridging, how good is the alignment
between board and stencil? (printing between the pads?) Also, stepped
stencils sometimes have a tendency to not be really flat everywhere, due to
stress variations in thin versus thick areas (solder creeping under the
stencil). When pressing lightly with the back of a pencil on the stencil in
the questionable areas when placed on the board, does it feel like the
stencil is making solid contact?
Are the stepped areas to get thin areas or to get thick areas? How are the
steps manufactured? Chemically, laser ablation, glued on sections?
If you like, you can contact me directly at [log in to unmask]
Ahne.
-----Original Message-----
From: Steve Gregory [mailto:[log in to unmask]]
Sent: 23 November, 2012 21:55 PM
To: [log in to unmask]; [log in to unmask]
Subject: Re: [TN] Stencil Life...
Hi Ahne,
I know that "it depends". I was just looking for what can be expected from a
stencil as long as it hasn't been dinged, and the mesh is still intact and
the stencil is taut.
The reason that I'm asking is that we have a stencil that has been used many
times (probably around 10,000 prints or more) and we're having trouble with
bridging on some tiny QFN footprints in the stencil. It's a stepped stencil
because we have to place some RF fences around the most populated areas on
the board and that's at 7-mils, and the inside area is stepped down to
5-mils. There probably has been some extra pressure put on the stencil in
order to get the step to work. I can see the outline of the board coined
into the stencil. I think it's time to get a new stencil and just wanted to
know if expecting the stencil to last more than around 10,000 prints is
asking a lot...
Steve
P.S. I did think about how to spell Bob's last name for a bit and almost
spelled it with a "J", but then changed it to a "G"...
-----Original Message-----
From: [log in to unmask]
Sent: Friday, November 23, 2012 1:42 PM
To: [log in to unmask] ; [log in to unmask]
Subject: FW: [TN] Stencil Life...
Short answer: Yes, why not.
Long answer: It depends...........how the stencil is treated. If you use the
proper squeegee pressure, if you clean it well regularly, if you don't drop
tools on it, if you don't bang it against hard objects, you don't use a
screwdriver to clean apertures, etc.
I have seen stencils returned where I could see the pattern of runs of the
circuit board pressed into the stainless steel. Obviously the squeegee
pressure had been too high. Some came back with tears in the mesh (and in my
eye) and many times you could find dings and dents in the metal. So, misuse
is the worst enemy of a long stencil life.
Ahne.
PS: It's Bob Jillings, was CEO
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of steve gregory
Sent: 22 November, 2012 19:28 PM
To: [log in to unmask]
Subject: [TN] Stencil Life...
Hi all!
First, let me wish everyone a happy Thanksgiving. I think that all of us can
sit back and be thankful for something in our lives, no matter how small it
is, and that's what this day is all about.
Now to my question; how long, or what is the useful life of a stainless
steel stencil? I know there is a lot of "It depends" that will figure into
the answer. But seem to recall someone telling me that a stencil should last
for 10,000 prints...I think I remember Bob Gillings of SMT (before Alpha
bought him out) telling me that.
What do you think? Should a stencil last that long?
Steve
Sent via BlackBerry by AT&T
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|