Agree. Was using 5 degree before.
Joyce Koo
Materials Researcher - Materials Interconnect Lab
Research In Motion Limited
Office: (519) 888-7465 79945
Mobile: (226) 220-4760
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Vladimir Igoshev
Sent: Wednesday, November 28, 2012 1:01 PM
To: [log in to unmask]
Subject: Re: [TN] Delta Tg on a Pb-free board.
A "magic" number within the industry is 5-6 C, unless I'm completely out to lunch.
Regards,
Vladimir
SENTEC Testing Laboratory Inc.
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
-----Original Message-----
From: "Honsowetz, Eric" <[log in to unmask]>
Sender: TechNet <[log in to unmask]>
Date: Wed, 28 Nov 2012 12:50:51
To: <[log in to unmask]>
Reply-To: TechNet E-Mail Forum <[log in to unmask]>,
"Honsowetz, Eric"
<[log in to unmask]>
Subject: Re: [TN] Delta Tg on a Pb-free board.
Yes - this is not an area of expertise for me - I have seen reports that suggest that under a 2% change in Tg would be a number...
eric
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Vladimir Igoshev
Sent: Wednesday, November 28, 2012 12:05 PM
To: [log in to unmask]
Subject: Re: [TN] Delta Tg on a Pb-free board.
One should keep in mind that the method doesn't specify a pass/fail number!?
Regards,
Vladimir
SENTEC Testing Laboratory Inc.
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
-----Original Message-----
From: Victor Hernandez <[log in to unmask]>
Sender: TechNet <[log in to unmask]>
Date: Wed, 28 Nov 2012 10:55:11
To: <[log in to unmask]>
Reply-To: TechNet E-Mail Forum <[log in to unmask]>,
<[log in to unmask]>
Subject: Re: [TN] Delta Tg on a Pb-free board.
Eric,
Thanks for sharing. This shared Test Method will test for laminate properly cures to specifications. Now the question is. Is there a Test Method for evaluating the woven fiber glass cloth adhesion property to the resin system,?
"X"
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Honsowetz, Eric
Sent: Wednesday, November 28, 2012 8:35 AM
To: [log in to unmask]
Subject: Re: [TN] Delta Tg on a Pb-free board.
IPC-TM-650 2.4.25
eric
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Victor Hernandez
Sent: Wednesday, November 28, 2012 7:30 AM
To: [log in to unmask]
Subject: Re: [TN] Delta Tg on a Pb-free board.
Board guru,
Is there a test method, IPC Standard, for testing how well a laminate has been cured, IS415.
"X"
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Zweig
Sent: Tuesday, November 27, 2012 4:11 PM
To: [log in to unmask]
Subject: Re: [TN] Delta Tg on a Pb-free board.
On Nov 27, 2012, at 4:46 PM, "Vladimir Igoshev. PhD" <[log in to unmask]> wrote:
> Hello board gurus,
>
> We ran a DSC test on a Pb-free PWB and found that Tg1 was around 172C,
> while the second heating produced Tg at about 185C. Below is a reply
> from the board vendor, stating that there is no such a thing as
> undercured laminate for that specific type of material.
>
> I'd greatly appreciate any constructive comments.
>
> "...That type of delta Tg would only apply to dicy materials when Tg1 and Tg2 are less than the advertised Tg of the material.
> EM-827 is a high Tg, filled phenolic and as such for these type phenolics, there is no delta Tg that signifies undercure.
> With filled phenolics like this both the Tg1 and Tg2 would be under the advertised Tg to be undercure and this is not the case.
> As you cure more and more these type phenolics both Tg1 and Tg2 move
> to higher and higher values and the delta Tg remains about the same".
>
>
> --
> Best regards,
>
> Vladimir Igoshev. PhD mailto:[log in to unmask]
>
> SENTEC Testing Laboratory Inc.
> 11 Canadian Road, Unit 7.
> Scarborough, ON M1R 5G1
> Tel: (416) 899-1882
> Fax: (905) 882-8812
> www.sentec.ca
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]
> ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
**********************
** LEGAL DISCLAIMER **
**********************
This E-mail message and any attachments may contain legally privileged, confidential or proprietary information. If you are not the intended recipient(s), or the employee or agent responsible for delivery of this message to the intended recipient(s), you are hereby notified that any dissemination, distribution or copying of this E-mail message is strictly prohibited. If you have received this message in error, please immediately notify the sender and delete this E-mail message from your computer.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
**********************
** LEGAL DISCLAIMER **
**********************
This E-mail message and any attachments may contain
legally privileged, confidential or proprietary
information. If you are not the intended recipient(s),
or the employee or agent responsible for delivery of
this message to the intended recipient(s), you are
hereby notified that any dissemination, distribution
or copying of this E-mail message is strictly
prohibited. If you have received this message in
error, please immediately notify the sender and
delete this E-mail message from your computer.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|