Our stainless soldering application was a drain wire on a thin stainless foil for a transformer shield. The special flux was VERY active and required lots of washing to neutralize the flux. We soldered it with 63/37 or SAC305 I think. Oh, that is interesting... We don't have any 63/37 or SAC305 that is not cored with flux. So it sounds like we were actually creating quite the chemistry project. Starting research and testing with non-flux core solder.
Thanks for triggering a wake-up call.
Phil
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Goodyear, Patrick
Sent: Monday, October 01, 2012 11:06 AM
To: [log in to unmask]
Subject: Re: [TN] soldering stainless steel
When we solder stainless we typically silver solder or silver braze the stainless, possible solution would be to silver braze a pad on the stainless then solder using Sn-Pb to the board.
Pat
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Paul Edwards
Sent: Friday, September 28, 2012 2:12 PM
To: [log in to unmask]
Subject: Re: [TN] soldering stainless steel
Should be able to solder directly to iron in S/S as long as there is no thick passivation layer or surface chemical enhancement....
Paul
Paul Edwards
Process/Quality Engineering
Surface Art Engineering
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Victor Hernandez
Sent: Friday, September 28, 2012 10:33 AM
To: [log in to unmask]
Subject: Re: [TN] soldering stainless steel
Perhaps a nickel under plate?
Victor,
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of McGrath, Jim
Sent: Friday, September 28, 2012 12:00 PM
To: [log in to unmask]
Subject: Re: [TN] soldering stainless steel
Preplate the solder area with Sn or SnPb. You may need a copper underplate.
Jim McGrath
Strategic Marketing Manager
TE Consumer Devices
Cell: 630-244-3872
Email: [log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Torsten Hagge
Sent: Friday, September 28, 2012 10:17 AM
To: [log in to unmask]
Subject: [TN] soldering stainless steel
Hi all,
has anybody experience with soldering stainless steel parts directly on a PCB? What solder process work fine?
Application is a medical sensor with body contacts.
Torsten
Kind regards
KRISTRONICS GmbH
Torsten Hagge
Gewerbegrund 5-9
24955 Harrislee
Telefon +49 (0) 461 7741-624
Telefax +49 (0) 461 7741-642
[log in to unmask]
www.kristronics.de
Meet at electronica 2012, A6, 409
Gerichtsstand Flensburg, Handelsregister: HRB 1433 FL Geschäftsführer Dipl.-Ing. oec. Thormod Ohm Ust-Id-Nr. DE 811182059
Bankverbindung: Deutsche Bank AG Flensburg, Konto-Nr. 4216610, BLZ 21570011
IBAN: DE32 2157 0011 0421 6610 00, BIC: DEUT DE HH 215
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
PG&E is committed to protecting our customers' privacy.
To learn more, please visit http://www.pge.com/about/company/privacy/customer/
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
Note: All the information contained in this e-mail and its attachments is proprietary to Kaiser Systems, Inc. and it may not be reproduced without the prior written permission of sender. If you have received this email in error, please immediately return it to sender and delete the copy you received.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|