Paul,
Just to clarify, Phil is not attempting to "fix" a PWB or CCA that is already delaminated by baking it. He is contemplating adding a pre-bake in his process prior to assembly and reflow to remove the moisture that leads to delamination during subsequent reflow processes.
Most of the client companies I work for or communicate with, we pre-bake all PWBs at 105 deg. C. no vacuum, no nitrogen, just prior to assembly and reflow. The PWBs have differing bake durations based on moisture removal studies as detailed in IPC 1601.
If the PWBs cannot be immediately processed after baking, they go into a drybox until ready for processing.
In the 9 years since I have been here at GD, we have never had a delamination occur during reflow or hot gas rework. Not once. In the client companies I work for who utilize this practice, delaminations are very few and far between, perhaps 15 in 30 years that I am aware of. When they do happen, it has always been attributed to a bad PWB lot or has been found to be a prepreg issue, typically resin skips.
So should everybody jump up and add a pre-bake to their process? The answer is (ka-ching) it depends. If the CCA cost is so little and the existing number of delams that occur is so low (with no pre-bake as part of the existing process), then probably not. While some "aging" of the pads and plated through holes occurs, I have found the additional DPMO as a result of baking to be so low it does not show up except for on PWBs with immersion tin finish. And I do not use that finish.
However, I bake for no more than is necessary to remove the PWB moisture level to less than 20% of saturated moisture content, per IPC 1601. Some PWBs require only two or three hours at 105 C to obtain this level. Most require between 6 and 8 hours, and a few more massive (backplanes) require up to 12 hours.
Even a 36" by 40" PWB that was 48 layers and is .240" thick did not require more than 14 hours to get to less than 20%. Those cost $125K APIECE.
Would you want to take a chance with delamination on something like that?
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Paul Reid
Sent: Wednesday, August 15, 2012 12:55 PM
To: [log in to unmask]
Subject: Re: [TN] bare board pre-bake parameters
I always have to warn those who bake to get rid of delamination that it rarely works. The delamination will probably still be with you after the bake.
How do you know that you have delamination? Is it visible?
Sincerely,
Paul Reid
Program Coordinator
PWB Interconnect Solutions Inc.
235 Stafford Rd., West, Unit 103
Nepean, Ontario Canada, K2H 9C1
613 596 4244 ext. 229
Skype paul_reid_pwb
[log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Phil Nutting
Sent: August 15, 2012 10:40 AM
To: [log in to unmask]
Subject: [TN] bare board pre-bake parameters
Good morning all,
We have recently had some boards delaminate and are considering pre-baking as a possible solution. I need to know some "rules of thumb"
for pre-bake time and temperature, suggested atmosphere (dry nitrogen?), allowable time between pre-bake and soldering.
At the moment I only have minimal information on the boards so I don't know their physical size, number of layers or if they are SMT or PTH.
I realize it could be a bad batch and the problem may only be with one group of boards as this is not a common problem with boards form many of our fab houses or CMs.
Thanks in advance,
Phil Nutting
Design for Manufacturing Engineer
Kaiser Systems, Inc.
126 Sohier Road
Beverly, MA 01915
Phone: 978-922-9300 x1310
Fax: 978-922-8374
e-mail: [log in to unmask]<mailto:[log in to unmask]>
www.kaisersystems.com<http://www.kaisersystems.com>
www.linkedin.com/in/philnutting<http://www.linkedin.com/in/philnutting>
________________________________
Note: All the information contained in this e-mail and its attachments is proprietary to Kaiser Systems, Inc. and it may not be reproduced without the prior written permission of sender. If you have received this email in error, please immediately return it to sender and delete the copy you received.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|