TECHNET Archives

August 2012

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Goodyear, Patrick" <[log in to unmask]>
Date:
Wed, 15 Aug 2012 15:47:18 +0000
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Whittaker, Dewey (EHCOE)" <[log in to unmask]>
Message-ID:
Subject:
From:
"Whittaker, Dewey (EHCOE)" <[log in to unmask]>
MIME-Version:
1.0
In-Reply-To:
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="us-ascii"
Parts/Attachments:
text/plain (226 lines)
Now we're getting there. Did the part actually fail or did the test indicate circuit failure? Some resistors when used at 50% fail tolerance limits and suffer degradation. Some resistors due to the SMT assembly nature have leakage paths that due to their design stress other components which will either fail the test or eventually the resistor itself. The component test is easy once removed in a non-contributory process. Looks for cracks and things as mentioned. Visually examine the PB surface between the pads once the component has been removed. . Clean the surface and either put the old part back on if you feel it is acceptable or a new one with a process that is benign as possible (minimum paste/flux to minimize deposition of contaminates between the PB and component substrate between the pads) and
re-run the tests to verify potential component/substrate/process failure mechanisms.
Dewey


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Goodyear, Patrick
Sent: Wednesday, August 15, 2012 8:15 AM
To: [log in to unmask]
Subject: Re: [TN] Intermittent single part failure

Might want to try a dye penetrant test similar to what they use in metallurgy testing to reveal any micro cracking that might be occurring that cannot be seen with available means.  

Pat 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: Wednesday, August 15, 2012 8:08 AM
To: [log in to unmask]
Subject: Re: [TN] Intermittent single part failure

GOOD question, Joyce!
Along with that, the de-rating of the chip resistor should be taken into account when doing a root cause analysis of the failure.

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo
Sent: Wednesday, August 15, 2012 9:58 AM
To: [log in to unmask]
Subject: Re: [TN] Intermittent single part failure

Assume it is not chip resistor (based on discoloration statement - hard to see chip resistor color difference) - are you sure you not over stress the resistor by design?  

Joyce Koo
Materials Researcher - Materials Interconnect Lab Research In Motion Limited
Office: (519) 888-7465 79945
Mobile: (226) 220-4760


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Victor Hernandez
Sent: Wednesday, August 15, 2012 10:47 AM
To: [log in to unmask]
Subject: Re: [TN] Intermittent single part failure

Hot and cold spray while conducting Rx measurement.

Victor,

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Chris Mahanna
Sent: Wednesday, August 15, 2012 9:40 AM
To: [log in to unmask]
Subject: Re: [TN] Intermittent single part failure

I agree with Paul, Mike and Bruce

There is art form to designing failure analysis that doesn't destroy evidence and end-up "no trouble found".

My best guess is a resistor fracture defect that requires mechanical stress to be patent at room conditions.
Reflow relieves the stress.
Microsection or isolation resistance at elevated T/H should be able to discover the failure mode.

Chris

Chris Mahanna
Robisan Laboratory
317-353-6249
 


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Bruce Tostevin
Sent: 2012/08/15 10:08 AM
To: [log in to unmask]
Subject: Re: [TN] Intermittent single part failure

Hello Michael,

You mentioned "aside from some slight discoloration." Something has to have caused that if it's unique to the failed parts. The component's thermal, chemical, airflow pattern,  and environmental exposures all need to be investigated. 

In summary notes 4 and 5, the failure was "cleared" by reheating R37
which properly measured 49.9Kohm after it was removed.   I suggest that
next time you have a confirmed failure, DO NOT reheat the part or use soldering irons/talons to remove it.  Instead, remove it by slowly and carefully digging away the solder joints with a sharpened pick or graver. Practice first on a scrap card until you get the technique down.
With this method  you can measure its value "as is" on the card without the influence of reflowing the joints.  If the resistor is defective then you can pursue that avenue of analysis.  At the same time you'll be able to inspect the component underside and the pcb location for signs of contamination, residues, etc. You're sure that nobody's doing any "hand" touch-up at this location?

Bruce Tostevin
Benchmark Electronics
Nashua, NH
 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Kuczynski, Michael (H USA)
Sent: August 14, 2012 2:24 PM
To: [log in to unmask]
Subject: [TN] Intermittent single part failure

We're experiencing a consistent intermittent (if such a thing?), contact failure for a single resistor (about 5% of 3K pcbs) . There are 2 of the same resistor on the PCB, yet just the one always has failure. Poor solder joints or voiding don't seem to be the issue, as I'd expect other failures elsewhere on the board. Aside from some slight discoloration, we're kinda puzzled. Even the measurements of the signals on the boards don't point to a path to look at.

Anyone have an opinion on a different angle we can try to look at?
Thanks in Advance.

SIEMENS
Michael Kuczynski      Healthcare Diagnostics Inc.
Product Eng. II CID      511 Benedict Ave.
914-524-3118 (Ph)       Tarrytown, NY 10591
914-524-3322 (Fax)      Mail Stop P25-1-C
[log in to unmask]<mailto:[log in to unmask]>


Here's a summary of our findings to date,


1.       We re-test the assembly on receipt and confirmed the failure.
The assembly originally recorded a pass when first manufactured.

2.       R37 and the adjacent components were X rayed and viewed under
high magnification and showed no signs of heat damage or physical damage. The solder fillet conforms to IPC standards. See pictures below
(removed) ,


3.       The SMT profile was re-ran and confirmed to be within
specification.

4.       We have re-created the effect described in your email -  by
touching up the solder joint at R37 the fault cleared.

5.       R37 was removed and resistance measured at 49.9K ohms, the
component was re-examined and showed in signs of physical damage.

6.       R37 was refitted and the board passed test.

7.       The range of serial number suggest the problem isn't batch
related having date codes from Week 25 Year 09 to Week 09 Year 12.

We will look at the other board when it arrives but at the moment we cannot draw any conclusions to the cause of these failures.



 
WET/DRY
                     S1_SIG        S2_SIG:         S1_REF:
S2_REF.:
S/N:             TP25:             TP24:              TP23:
TP26:             FINDINGS:
COMMENTS:
57901011     4.53 / 2.18     4.64 / 2.05          3.5
3.5                 WORKS                                           *
88011123     4.53 / 2.18     4.65 / 2.06          3.5
3.5                 WORKS
11800925     4.50 / 2.15     (3.40 / 1.33)        3.5
3.5                 S2 SHOWED DRY WHEN WET         DOWN SHIFT OF S2
92661209     4.52 / 2.15     4.63 / 2.30         (2.4)
3.5
REFERENCE VOLTAGE S1 FELL
14270925     4.51 / 2.14     (2.31 / 0.90)        3.5
3.5                 S2 SHOWED DRY WHEN WET         DOWN SHIFT OF S2**
91021147     4.50 / 2.14     4.60 / 2.02          3.5
(3.5 / 4.1)***
REF. VOLTAGE S2 ROSE EVEN ISOLATED FROM COMPARATOR
93511209     4.50 / 2.20     (1.57 / 0.63)        3.5
(1.8)
SENT FOR ANALYSIS
15510925     4.45 / 2.05     4.62 / 2.04         (4.6)
3.49
RXD 8/8/12

* GOT QUESTIONABLE COMPARATOR
** LOST QUESTIONABLE COMPARATOR
*** INTERMITTENT


This message and any attachments are solely for the use of intended recipients. The information contained herein may include trade secrets, protected health or personal information, privileged or otherwise confidential information. Unauthorized review, forwarding, printing, copying, distributing, or using such information is strictly prohibited and may be unlawful. If you are not an intended recipient, you are hereby notified that you received this email in error, and that any review, dissemination, distribution or copying of this email and any attachment is strictly prohibited. If you have received this email in error, please contact the sender and delete the message and any attachment from your system. Thank you for your cooperation

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________



______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________



______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________

---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________


PG&E is committed to protecting our customers' privacy. 
To learn more, please visit http://www.pge.com/about/company/privacy/customer/

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2