TECHNET Archives

August 2012

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Date:
Wed, 15 Aug 2012 14:04:11 +0100
Reply-To:
Message-ID:
<4384FCCEBB3B4C2CB2E98EA724A698FB@MikeLaptop>
Subject:
From:
Mike Fenner <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (165 lines)
In a related vein.
Where on the PCB are the defective parts located? If they are too close to
an edge then they can be stressed on breakout leading to internal cracking
or joint failure. Alternatively/as well if you have too much solder giving
high fillets these can work like a vice and similarly over stress. 
If the component [joint] is cracked it could still pass a probe test as that
can "make" the connection. HIP can present in a similar way.



Regards

Mike 



-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Paul Reid
Sent: Wednesday, August 15, 2012 1:12 PM
To: [log in to unmask]
Subject: Re: [TN] Intermittent single part failure

I would look at intermittent board defects. 

Microvias and butt joint failures produce intermittent board level
failures. See if the failure is brought on by heating and flexing the
board.


Paul Reid 

Program Coordinator  

PWB Interconnect Solutions Inc. 
235 Stafford Rd., West, Unit 103 
Nepean, Ontario Canada, K2H 9C1 

613 596 4244 ext. 229  

Skype paul_reid_pwb 
[log in to unmask] 

 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Kuczynski, Michael
(H USA)
Sent: August 14, 2012 2:24 PM
To: [log in to unmask]
Subject: [TN] Intermittent single part failure

We're experiencing a consistent intermittent (if such a thing?), contact
failure for a single resistor (about 5% of 3K pcbs) . There are 2 of the
same resistor on the PCB, yet just the one always has failure. Poor
solder joints or voiding don't seem to be the issue, as I'd expect other
failures elsewhere on the board. Aside from some slight discoloration,
we're kinda puzzled. Even the measurements of the signals on the boards
don't point to a path to look at.

Anyone have an opinion on a different angle we can try to look at?
Thanks in Advance.

SIEMENS
Michael Kuczynski      Healthcare Diagnostics Inc.
Product Eng. II CID      511 Benedict Ave.
914-524-3118 (Ph)       Tarrytown, NY 10591
914-524-3322 (Fax)      Mail Stop P25-1-C
[log in to unmask]<mailto:[log in to unmask]>


Here's a summary of our findings to date,


1.       We re-test the assembly on receipt and confirmed the failure.
The assembly originally recorded a pass when first manufactured.

2.       R37 and the adjacent components were X rayed and viewed under
high magnification and showed no signs of heat damage or physical
damage. The solder fillet conforms to IPC standards. See pictures below
(removed) ,


3.       The SMT profile was re-ran and confirmed to be within
specification.

4.       We have re-created the effect described in your email -  by
touching up the solder joint at R37 the fault cleared.

5.       R37 was removed and resistance measured at 49.9K ohms, the
component was re-examined and showed in signs of physical damage.

6.       R37 was refitted and the board passed test.

7.       The range of serial number suggest the problem isn't batch
related having date codes from Week 25 Year 09 to Week 09 Year 12.

We will look at the other board when it arrives but at the moment we
cannot draw any conclusions to the cause of these failures.



 
WET/DRY
                     S1_SIG        S2_SIG:         S1_REF:
S2_REF.:
S/N:             TP25:             TP24:              TP23:
TP26:             FINDINGS:
COMMENTS:
57901011     4.53 / 2.18     4.64 / 2.05          3.5
3.5                 WORKS                                           *
88011123     4.53 / 2.18     4.65 / 2.06          3.5
3.5                 WORKS
11800925     4.50 / 2.15     (3.40 / 1.33)        3.5
3.5                 S2 SHOWED DRY WHEN WET         DOWN SHIFT OF S2
92661209     4.52 / 2.15     4.63 / 2.30         (2.4)
3.5
REFERENCE VOLTAGE S1 FELL
14270925     4.51 / 2.14     (2.31 / 0.90)        3.5
3.5                 S2 SHOWED DRY WHEN WET         DOWN SHIFT OF S2**
91021147     4.50 / 2.14     4.60 / 2.02          3.5
(3.5 / 4.1)***
REF. VOLTAGE S2 ROSE EVEN ISOLATED FROM COMPARATOR
93511209     4.50 / 2.20     (1.57 / 0.63)        3.5
(1.8)
SENT FOR ANALYSIS
15510925     4.45 / 2.05     4.62 / 2.04         (4.6)
3.49
RXD 8/8/12

* GOT QUESTIONABLE COMPARATOR
** LOST QUESTIONABLE COMPARATOR
*** INTERMITTENT


This message and any attachments are solely for the use of intended
recipients. The information contained herein may include trade secrets,
protected health or personal information, privileged or otherwise
confidential information. Unauthorized review, forwarding, printing,
copying, distributing, or using such information is strictly prohibited
and may be unlawful. If you are not an intended recipient, you are
hereby notified that you received this email in error, and that any
review, dissemination, distribution or copying of this email and any
attachment is strictly prohibited. If you have received this email in
error, please contact the sender and delete the message and any
attachment from your system. Thank you for your cooperation

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask] 
______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________



______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2