Anil,
I agree the chemistries are sound and I am aware of some success stories. I was trying to stay mainstream with the reply.
Dewey
-----Original Message-----
From: Anil Kher [mailto:[log in to unmask]]
Sent: Thursday, August 16, 2012 12:20 AM
To: Whittaker, Dewey (EHCOE); [log in to unmask]
Subject: RE: PCB finish: ENIG vs. hard gold
Dewey
I would like to make a case for Electrolytic Gold on Nickel. It is a bit
costly. However you can assemble without a worry about black pad. It is the
only finish that will work well on a combination of fine pitch soldering +
selective pad/wiper contacts or Gold wire bond or aluminium wire bond. The
plus point is the Nickel is pure and the gold can be plated unalloyed
(though it includes carbonaceous material in the matrix - which has never
shown any ill effects). The plating was extensively used for PC plug in
cards/ for multimeter PCBs - by Fluke etc and today in automotive for wiper
/switch contacts and C.O.B
Anil Kher
-----Original Message-----
From: Whittaker, Dewey (EHCOE) [mailto:[log in to unmask]]
Sent: 15 August 2012 22:05
Subject: Re: PCB finish: ENIG vs. hard gold
Kevin,
Bob and Joyce made good points. Here is my ranking:
ˇ Bare copper with a TBD nano-technology OSP
ˇ ENEPIG
ˇ HAL with a TBD alloy (snick, etc.)
ˇ ENIGš
ˇ IAg
ˇ OSP
Note 1 - If you have a sufficient volume of business or very close
relationships that you feel you are getting their full attention and they
have a good history of process control, then this is a good selection.
Dewey
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Robert Kondner
Sent: Wednesday, August 15, 2012 9:09 AM
To: [log in to unmask]
Subject: Re: [TN] PCB finish: ENIG vs. hard gold
Kevin,
Add to that the monitoring of the ENIG. If the process is not controlled
you could end up with black pad or other soldering problems.
Bob K.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Glidden, Kevin
Sent: Wednesday, August 15, 2012 12:01 PM
To: [log in to unmask]
Subject: Re: [TN] PCB finish: ENIG vs. hard gold
Thank you, everyone, for your responses. To summarize (and ensure my
understanding is correct):
"Hard Gold" is essentially electroplated gold that is co-deposited with
other alloying metals (nickel and/or cobalt) to make it "hard". This
plating is primarily used for gold-finger edge card contacts, and not
soldering. Many responses indicated that due to the alloying metals,
these surfaces are not at all solderable.
The distinction is that "soft gold" or "gold flash" [which may be what the
PCB supplier actually meant to say] that is also electroplated can typically
be soldered to, but has some key disadvantages to ENIG, such as:
- the ENIG immersion gold process is self limiting and as such results in a
uniform plating thickness, whereas the electroplated gold final thickness is
dependent on many factors such as plating chemistry cleanliness, geometry,
current density, processing time, etc, etc. The concern is that too much
gold can cause gold embrittlement of the solder joints (weak solder joints)
as the gold itself "dissolves" into the solder joint mass during the
soldering process. The max thickness recommended is 4 to 8 microinches
(vs typical 3-5 microinches for ENIG), which requires strict process
control.
- the ENIG process results in better uniformity, whereas the electroplated
gold has a higher porosity, which in turn can result (particularly at
thinner deposit thickness) with less protection for solderability, reduces
shelf life, etc.
- the ENIG process results in higher purity gold, as it is chemically
induced. The electroplated gold typically has a lower purity as other
conductive metals can co-plate in solution.
- the ENIG immersion gold process results in gold plating over the pad edges
as well as the lands, whereas the elctroplated covers only the lands and
would leave bare copper on the pad edges.
Based on these points and the responses, it seems ENIG is the better and
safest choice.
From: Glidden, Kevin
Sent: Tuesday, August 14, 2012 12:12 PM
To: [log in to unmask]
Subject: PCB finish: ENIG vs. hard gold
Hi everyone,
We have a PCB supplier who is offering "Hard Gold" as an alternate to ENIG
finish, due to PCB size and processing capabilities. The application is
Class 3 (mil/aero). The circuit is thin FR4 and subject to SMT reflow w/
Sn63Pb37 (non RoHS) solder alloy, and moderate flexing in end application.
Can anyone offer info on the differences between the two finishes, and/or
their suitability? Is there an IPC spec (or specs) that outline "hard
gold"?
Thanks,
Kevin Glidden
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|