TECHNET Archives

June 2012

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Gumpert, Ben" <[log in to unmask]>
Date:
Fri, 29 Jun 2012 13:13:50 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Message-ID:
Subject:
From:
"David D. Hillman" <[log in to unmask]>
X-cc:
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (113 lines)
Hi folks! We have had the same success as Ben detailed. Our maximum void 
requirement is 50% of the pad and by using the window pane approach, we 
typically are getting 70%-80% coverage. We have had only two instances 
were we needed better coverage due to either a  component thermal or a 
grounding issue. We still used the window pane approach but had to conduct 
a series of DOEs to achieve the required coverage. 

And welcome back Ed!

Dave Hillman
Rockwell Collins
[log in to unmask]



"Gumpert, Ben" <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
06/29/2012 12:15 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Gumpert, Ben"  <[log in to unmask]>


To
<[log in to unmask]>
cc

Subject
Re: [TN] I'm back and have a question about QFN voids






Ed,

I'm interested to see what result you get with wave soldering, but I worry 
about e-mail access where you are going.

I've had good success with minimizing voids on QFNs by using a window-pane 
(array of apertures) on the center pad. I aim for 50% coverage of the 
center pad area. But you have to make sure that your signal pins can 
accommodate - either the solder paste reduction has to be the same for 
bottom only terminations, or you need a larger PCB pad (extending out from 
under the part) for excess solder to flow (so that the center pad solder 
determines the offset height of the part, not the perimeter solder 
joints.)

Ben

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ed Popeielarski
Sent: Friday, June 29, 2012 12:52 PM
To: [log in to unmask]
Subject: EXTERNAL: [TN] I'm back and have a question about QFN voids

Greetings 'netters,

For the past 2 1/2 years I've been lurking because Technet didn't get 
along with my employer's email system (specifically during maintenance).

I solved that problem by finding another employer! See how much you guys 
mean to me?!

It's good to be "back in the saddle again", so please allow me to begin 
with a perplexing question:

I need to solve QFN ground-pad voiding on a 0.038" thick ENIG assembly. 
The application is a high power RF amp and voiding as low as 25% causes 
issues with reliability.

Many attempts to resolve this with stencil variations, (thickness, star 
patterns, etc) and process variables (reflow time/temps) have been 
fruitless.

I'm considering re-spinning the board with a via dead center of this 6mm 
part, print & reflow only the leads, then wave solder the via (SAC305 with 
water soluble flux) in hopes of forcing the volatiles out from the center 
due to the wetting forces. Has anyone tried and succeeded with this method 
or am I sailing off the edge of the planet?

Thanks for your help in advance.


Ed Popielarski
Engineering Manager

Technical Services, Inc.
970 NE 21st Ct.
Oak Harbor, Wa. 98277

Ph: 360-675-1322
Fx: 206-624-0965
Cl: 949-581-6601

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________



______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2