Craig,
Was this PCB/ connector subjected to wave solder, hand solder and or
intrusive pin/paste solder process?
I have seen touch up soldering to " fill the barrel" on the component side
create voids and contaminant entrapment which may be a reliability issue.
What is the cumulative fill? Solder fill provides the mechanical strength
to withstand its service environment.
Eva
Spec Tech
On Wed, May 16, 2012 at 9:12 AM, David D. Hillman <
[log in to unmask]> wrote:
> Hi Craig! One of the downsides of now having access to Xray inspection
> technology is that we can see many "things" we never could before - which
> now causes the question "is that bad?". There is currently no plated thru
> hole void criteria in the IPC JSTD 001 specification. I would recommend
> that an assessment of the assembly be initiated. Pulling and inspecting a
> number of assemblies that either have been in the field or have passed all
> of the qualification tests will demonstrate what level of voids typically
> exist and if that level of voiding is a reliability issue. The presence of
> voids is not necessarily an indication of a reliability issue. Good Luck.
>
> Dave Hillman
> Rockwell Collins
> [log in to unmask]
>
>
>
> Craig Sullivan <[log in to unmask]>
> Sent by: TechNet <[log in to unmask]>
> 05/16/2012 07:14 AM
> Please respond to
> TechNet E-Mail Forum <[log in to unmask]>; Please respond to
> Craig Sullivan <[log in to unmask]>
>
>
> To
> <[log in to unmask]>
> cc
>
> Subject
> [TN] Through hole barrel voids
>
>
>
>
>
>
> Hi everyone,
>
>
>
> We have a certain board with several through hole connectors. The customer
> has provided us x ray images showing voiding in the barrels. Fillets on
> both
> sides are acceptable, and the solderability tests are ok. This seems to be
> isolated to this board because random sampling on other boards shows
> virtually no voiding. The only voiding "criteria" I can find is related to
> BGAs. Is there any published criteria / reference material for this type
> of
> defect?
>
>
>
> Thank you,
>
> Craig Sullivan
>
> Manufacturing Engineer
>
> MPL Incorporated
>
> P: 607.266.0480
>
> F: 607.266.0482
>
> <mailto:[log in to unmask]> [log in to unmask]
>
> P Please consider the environment before printing this e-mail.
>
>
>
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
>
>
> ______________________________________________________________________
> This email has been scanned by the Symantec Email Security.cloud service.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|
|
|