Thanks for the support.
Now we need the guys in charge of 6012 to agree.
Paul Reid
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Thayer, Wayne - IIW
Sent: April 17, 2012 3:27 PM
To: [log in to unmask]
Subject: Re: [TN] Micro Stacked Via, solid copper plating, voiding
I agree with you Paul. Microvias must not have fluid filled voids.
Excellent examples.
Wayne Thayer
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Paul Reid
Sent: Thursday, April 12, 2012 4:04 PM
To: [log in to unmask]
Subject: Re: [TN] Micro Stacked Via, solid copper plating, voiding
Hi Denny,
This was a layer1/2 microvia that is supposed to be copper filled with a
cap layer also. The microvia is on a buried via I believe but I don't
remember It could be on another microvia. The section is to the center
of the microvia.
What we did was we preformed an IST test and this microvia failed in 19
cycles. The failure is a 10% increase in resistance.
Sincerely,
Paul Reid
Program Coordinator
PWB Interconnect Solutions Inc.
235 Stafford Rd., West, Unit 103
Nepean, Ontario Canada, K2H 9C1
613 596 4244 ext. 229
Skype paul_reid_pwb
[log in to unmask]
________________________________
From: Dennis Fritz [mailto:[log in to unmask]]
Sent: April 12, 2012 1:53 PM
To: [log in to unmask]; Paul Reid
Subject: Re: [TN] Micro Stacked Via, solid copper plating, voiding
Paul,
I am having a bit of a problem understanding what this construction was.
Obviously layer 1 to layer 2. But there seems to have been some cap
plating at layer 2. Also, the microvias seem an a very high aspect
ratio. They surely were sectioned to the center of the microvia? Did
the cracks you point out show up as opens or intermittents? You must
have cycled these to be sectioning them, surely those are not knit lines
from copper plating.
Guess a little background on these would help the analysis. Thanks -
Denny Fritz
-----Original Message-----
From: Steve Gregory <[log in to unmask]>
To: TechNet <[log in to unmask]>
Sent: Thu, Apr 12, 2012 9:04 am
Subject: Re: [TN] Micro Stacked Via, solid copper plating,
voiding
Hi Paul!
Sorry I didn't get your photos posted yesterday, got rather busy
yesterday,
but I have them posted now:
http://stevezeva.homestead.com/MV_Void_with_Barrel_Crack_01.jpg
http://stevezeva.homestead.com/MV_Void_with_Barrel_Crack_02.jpg
http://stevezeva.homestead.com/MV_Void_with_Barrel_Crack_03.jpg
http://stevezeva.homestead.com/MV_Void_with_Barrel_Crack_06.jpg
http://stevezeva.homestead.com/MV_Void_with_Crystal_01.jpg
http://stevezeva.homestead.com/MV_Void_with_Crystal_02.jpg
Steve
-----Original Message-----
From: Paul Reid [mailto:[log in to unmask]
<mailto:[log in to unmask]> ]
Sent: Wednesday, April 11, 2012 3:06 PM
To: TechNet E-Mail Forum; [log in to unmask]
Subject: RE: [TN] Micro Stacked Via, solid copper plating, voiding
Hi Victor,
I do not know that this is covered by IPC documents or not but I know
that
it can be a problem.
Microvia voids have typically been acceptable if you do not violate the
minimum thickness requirement of the copper in the barrel of the hole.
What we have is an enclosed void that has plating solution in the void
by
default. The void cannot be plating closed without solution being
trapped in
the void. This makes the void very susceptible to conductive anodic
filament
(CAF) type of failure if there is a crack the goes to the void. I spent
years looking for that crack and finally found one.
Most voids do not produce a crack but on two occasions I have found
cracks
into voided microvias.
It is why I suggest that voids be avoided in any high end application.
It is not a standard but it is my take on this problem. Voids in plated
closed microvias should not be allowed is my suggestion to the 6012
committee.
I have sent pictures to Steve Gregory to post on his web site. You'll
note
the plated closed microvias voids with cracks in the barrel on the
microvia.
In two pictures you will see a blue crystal that is still in the
microvia
that is from the plating solution. It is rare to find the blue crystal
because microsectioning flushes out the blue crystals during processing.
Sincerely,
Paul Reid
Program Coordinator
PWB Interconnect Solutions Inc.
235 Stafford Rd., West, Unit 103
Nepean, Ontario Canada, K2H 9C1
613 596 4244 ext. 229
Skype paul_reid_pwb
[log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask] <mailto:[log in to unmask]> ] On
Behalf Of Victor Hernandez
Sent: April 11, 2012 11:14 AM
To: [log in to unmask]
Subject: [TN] Micro Stacked Via, solid copper plating, voiding
Fellow TechNetters:
I have searched for IPC documentation and/or Inductry Standards
concerning the acceptance/guidelines for solid plated micro via voidibg.
I did not locate any. Can someone confirm that and/or provided guidance
as
to which document covers that anomaly.
Victor,
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
This e-mail and any files transmitted with it may be proprietary and are
intended solely for the use of the individual or entity to whom they are
addressed. If you have received this e-mail in error please notify the
sender.
Please note that any views or opinions presented in this e-mail are
solely those of the author and do not necessarily represent those of
Exelis Inc. The recipient should check this e-mail and any attachments
for the presence of viruses. Exelis Inc. accepts no liability for any
damage caused by any virus transmitted by this e-mail.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|