I sincerely doubt any Si in the solder, Probably the Si you are seeing is
from silica filler in the device body or something like that.
So what is happening to stop solder re-melting?
Possibly if the device leads are copper then with extended heating the Cu
can dissolve into the near pure Sn solder and drive the liquidus up - and
the longer you heat the greater the Cu dissolution and the higher the MP.
You are probably dissolving out the PCB pad/through hole barrel as well.
The Cu/Sn phase diagram looks like a tick or check mark. The short Sn down
stroke side is from 232 to low point of 227 and the Cu up stroke side is
near vertical to MP of Cu somewhere over 1000C, so you get a very rapid temp
increase for small compositional change.
Suggest try come in with a hot iron (more than 700) to melt out the existing
composition quickly or flush with more solder to add tin to the mix and
depress MP. Or both.
Regards
Mike Fenner
Bonding Services & Products
T: +44 [0] 1865 522 663 E: [log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: Tuesday, March 27, 2012 10:01 PM
To: [log in to unmask]
Subject: Re: [TN] Rework Concern and Question
I think, but am not sure, that you are attempting to remove a new component
whose leads are FINISHED (not soldered) with SAC305 solder, and that is why
you measure Sn98 on the parts straight out of the tape (I am going to
disregard the SEM analysis of 2% silicon for a moment).
Secondly, the new parts were probably soldered to the PWB with SAC305 solder
as well, and that is why when you attempt to unsolder them or bring them
into liquidus, you are having more difficulty than you did with the old
parts.
Not only were the old parts finished with Sn63 solder, but they were also
soldered in place with Sn63 solder.
The new parts are meant to be RoHS compliant, and apparently they are, with
a Sn level of 98%, and no Pb in sight on the SEM diagram. If that were the
only change, you should notice no difference in the ability to remove the
part if they were, in fact, soldered to the PWB with Sn63; the plating
change alone would not make any noticeable difference.
Soldering them to the PWB with lead-free SAC305 alloy would make a huge
difference in your ability to unsolder and remove the part, no matter what
finish was used to plate the part.
Silicon will not break down and become part of an alloy under 1000 deg. C.
The 2% SEM pickup is probably silicon chips or dust from the component body.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M.
Sent: Tuesday, March 27, 2012 3:25 PM
To: [log in to unmask]
Subject: Re: [TN] Rework Concern and Question
Dave Hillman,
With your metallurgical background you might be a better person than I to
make a comment. I'm not sure I've even had or seen an occasion where
something dissolved in the bulk solder and increased the
melting/solidification temperature. Yes I've seen the leading edge of
solder as it flows and wets a surface dissolve metallization and freeze
because the local meting temperature changed but I've never seen that happen
to the bulk of a solder joint
Regards,
George
George M. Wenger
Senior Principal Reliability / FMA Engineer
Andrew Corporation - Wireless Network Solutions
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 Office (732) 309-8964 Mobile
E-mail: [log in to unmask]
-----Original Message-----
From: Leland Woodall [mailto:[log in to unmask]]
Sent: Tuesday, March 27, 2012 4:14 PM
To: TechNet E-Mail Forum; Wenger, George M.
Subject: RE: [TN] Rework Concern and Question
George,
It's been a long day, and maybe I'm not making myself too clear.
We're not being able to achieve a liquidus state with a 700 degree F
soldering iron. We're not trying to melt the lead, just the solder that's
holding it to the PCB. We're not accomplishing that with the new component,
so I'm thinking something has mixed with the solder joint and has raised the
resultant reflow temperature.
Leland
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M.
Sent: Tuesday, March 27, 2012 4:10 PM
To: [log in to unmask]
Subject: Re: [TN] Rework Concern and Question
Leland,
Am I missing something? I don't think it really matter that the lead base
material or lead surface finish is. What matters is the solder used to
attach the lead to the board. When you desolder a lead you don't melt the
lead you melt the solder.
Regards,
George
George M. Wenger
Senior Principal Reliability / FMA Engineer Andrew Corporation - Wireless
Network Solutions
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 Office (732) 309-8964 Mobile
E-mail: [log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Tuesday, March 27, 2012 4:05 PM
To: [log in to unmask]
Subject: Re: [TN] Rework Concern and Question
Hi Leland - I recommend you find out the lead base metal composition. If you
shot an SEM-EDS of the lead toe, you could be getting the Si from the base
metal composition and not part of the solder alloy composition.
Dave Hillman
Rockwell Collins
[log in to unmask]
Leland Woodall <[log in to unmask]> Sent by: TechNet <[log in to unmask]>
03/27/2012 02:52 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to Leland Woodall
<[log in to unmask]>
To
<[log in to unmask]>
cc
Subject
Re: [TN] Rework Concern and Question
Vladimir,
We analyzed raw components straight out of the tape and reel packaging.
The site selection was on the bottom side of the leads at the toe.
Leland
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of vladimir Igoshev
Sent: Tuesday, March 27, 2012 3:12 PM
To: [log in to unmask]
Subject: Re: [TN] Rework Concern and Question
Sorry Ben, it doesn't.
Leland,
What you are saying sounds strange. What does it mean: "We've analyzed the
lead material beneath the SEM and it returns 98% tin and 2% silicone"? Did
you analyzed leads or solder? Where the analysis was taken from? Did you
analyzed leads with pads ripped off?
Regards,
Vladimir
SENTEC Testing Laboratory Inc.
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
-----Original Message-----
From: "Gumpert, Ben" <[log in to unmask]>
Sender: TechNet <[log in to unmask]>
Date: Tue, 27 Mar 2012 18:58:21
To: <[log in to unmask]>
Reply-To: TechNet E-Mail Forum <[log in to unmask]>,
"Gumpert, Ben"
<[log in to unmask]>
Subject: Re: [TN] Rework Concern and Question
Leland,
I won't claim to be an expert, but this website seems to imply something
along those lines.
http://resource.npl.co.uk/mtdata/phdiagrams/sisn.htm
Ben
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall
Sent: Tuesday, March 27, 2012 2:18 PM
To: [log in to unmask]
Subject: EXTERNAL: [TN] Rework Concern and Question
Folks,
We've ran across a strange incident and I'd like a little advice from the
group.
We recently underwent a component vendor change, and part of the first group
of boards were misbuilt due to incorrect polarity (the part marking was
misinterpreted by the vision operator).
Anyway, an attempt to remove the part by our Repair group resulted in lifted
pads on 10 of the first 12 boards. We've analyzed the lead material beneath
the SEM and it returns 98% tin and 2% silicone. The old style component
comes off quite easily (within 3 seconds), and an analysis of its leads
shows to be 100% tin. It's a 6 pin diode with very little mass.
What's going on here? Does a 2% silicone mix raise the melting point of
solder by 200 degrees C?
Please help me understand.
Thanks,
Leland
________________________________
?Confidentiality Notice:
This transmission (including any attachments) may contain confidential
information belonging to the sender and is intended only for the use of the
party or entity to which it is addressed. If you are not the intended
recipient, you are hereby notified that any disclosure, copying,
distribution, retention or the taking of action in reliance on the contents
of this transmission is strictly prohibited. If you have received this
transmission in error, please immediately notify the sender and erase all
information and attachments.?
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
________________________________
?Confidentiality Notice:
This transmission (including any attachments) may contain confidential
information belonging to the sender and is intended only for the use of the
party or entity to which it is addressed. If you are not the intended
recipient, you are hereby notified that any disclosure, copying,
distribution, retention or the taking of action in reliance on the contents
of this transmission is strictly prohibited. If you have received this
transmission in error, please immediately notify the sender and erase all
information and attachments.?
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
________________________________
"Confidentiality Notice:
This transmission (including any attachments) may contain confidential
information belonging to the sender and is intended only for the use of the
party or entity to which it is addressed. If you are not the intended
recipient, you are hereby notified that any disclosure, copying,
distribution, retention or the taking of action in reliance on the contents
of this transmission is strictly prohibited. If you have received this
transmission in error, please immediately notify the sender and erase all
information and attachments."
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|