Silicon/silicone can come as few sources: (a) mold release agent = silicone, (b) molding compound smear with silica filler - mold bleed. In addition, there are rheology adjustment agent used for the solder that might containing Si. And last, recycled cheap stuff might also have trace elements, including silicon.
Joyce Koo
Materials Researcher - Materials Interconnect Lab
Research In Motion Limited
Office: (519) 888-7465 79945
Mobile: (226) 220-4760
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall
Sent: Tuesday, March 27, 2012 3:53 PM
To: [log in to unmask]
Subject: Re: [TN] Rework Concern and Question
Vladimir,
We analyzed raw components straight out of the tape and reel packaging. The site selection was on the bottom side of the leads at the toe.
Leland
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of vladimir Igoshev
Sent: Tuesday, March 27, 2012 3:12 PM
To: [log in to unmask]
Subject: Re: [TN] Rework Concern and Question
Sorry Ben, it doesn't.
Leland,
What you are saying sounds strange. What does it mean: "We've analyzed the lead material beneath the SEM and it returns 98% tin and 2% silicone"? Did you analyzed leads or solder? Where the analysis was taken from? Did you analyzed leads with pads ripped off?
Regards,
Vladimir
SENTEC Testing Laboratory Inc.
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
-----Original Message-----
From: "Gumpert, Ben" <[log in to unmask]>
Sender: TechNet <[log in to unmask]>
Date: Tue, 27 Mar 2012 18:58:21
To: <[log in to unmask]>
Reply-To: TechNet E-Mail Forum <[log in to unmask]>,
"Gumpert, Ben"
<[log in to unmask]>
Subject: Re: [TN] Rework Concern and Question
Leland,
I won't claim to be an expert, but this website seems to imply something along those lines.
http://resource.npl.co.uk/mtdata/phdiagrams/sisn.htm
Ben
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall
Sent: Tuesday, March 27, 2012 2:18 PM
To: [log in to unmask]
Subject: EXTERNAL: [TN] Rework Concern and Question
Folks,
We've ran across a strange incident and I'd like a little advice from the group.
We recently underwent a component vendor change, and part of the first group of boards were misbuilt due to incorrect polarity (the part marking was misinterpreted by the vision operator).
Anyway, an attempt to remove the part by our Repair group resulted in lifted pads on 10 of the first 12 boards. We've analyzed the lead material beneath the SEM and it returns 98% tin and 2% silicone. The old style component comes off quite easily (within 3 seconds), and an analysis of its leads shows to be 100% tin. It's a 6 pin diode with very little mass.
What's going on here? Does a 2% silicone mix raise the melting point of solder by 200 degrees C?
Please help me understand.
Thanks,
Leland
________________________________
"Confidentiality Notice:
This transmission (including any attachments) may contain confidential information belonging to the sender and is intended only for the use of the party or entity to which it is addressed. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution, retention or the taking of action in reliance on the contents of this transmission is strictly prohibited. If you have received this transmission in error, please immediately notify the sender and erase all information and attachments."
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
________________________________
"Confidentiality Notice:
This transmission (including any attachments) may contain confidential information belonging to the sender and is intended only for the use of the party or entity to which it is addressed. If you are not the intended recipient, you are hereby notified that any disclosure, copying, distribution, retention or the taking of action in reliance on the contents of this transmission is strictly prohibited. If you have received this transmission in error, please immediately notify the sender and erase all information and attachments."
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|