Hi Sylvain - we have a couple of applications where we solder to manganin
wire and let's just say it not a fun task! You can use tin/lead solder but
the key is that you need a highly highly aggressive flux to deal with the
manganin surface oxides. I recommend you look at fluxes that are designed
for soldering stainless steel or magnet wire - Indium, Kester, Alpha,
etc. all of the solder suppliers offer flux formulations you can choose to
use. I would also recommend that the flux chemistry be a water soluble
formulation to aid in the removal of the flux residues/nonactivated flux
to avoid possible corrosion issues due to inadequate cleaning. Good luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
Sylvain Kaufmann <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
03/13/2012 09:18 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Sylvain Kaufmann <[log in to unmask]>
To
<[log in to unmask]>
cc
Subject
[TN] Soldering manganin wires?
Dear TechNetters,
One of our customer is designing and prototyping some cryogenic
temperatures measurement assemblies.
As part of the material used, the "temperature sensors" are supposed to be
connected to the PCB with manganin wires.
The PCB is a flex with ENIG finish.
I never heard about this material before and found it was an alloy mixing
86% copper, 12% manganese, 2% nickel.
I checked the TechNet archive as well as the internet, but was not
successful in finding guidelines about soldering those wires.
I found some words on NPL website about copper-manganese alloys : quote
from website -> Joints between the copper manganese alloys and copper are
made most effectively by welding in an atmosphere of argon, and by hard
soldering if welding is impracticable.
On the other hand, I found some papers from some physicists or some
hobbyist video stating that manganin can be soldered with regular tin-lead
solder (well, at least they did it on their proto apparatus)...
Provided I can find only very few info and mostly not consistent, I turn
my eyes on you experts out there.
Does anyone have experience in soldering this material?
Or more precisely, is this material solderable with some regular
electronic solder alloys?
As usual, thanks a lot in advance for your valuable input.
Kind regards
sylvain
--------------------------------------------------------------------------------------------------
Sylvain Kaufmann
CERN - European Laboratory for Particle Physics
Dpt : TE-MPE-EM
Office : 160/1-026
Tel : +41 22 767 37 02
Fax : +41 22 766 87 77
--------------------------------------------------------------------------------------------------
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|
|
|