Hi Wayne,
That's what we were thinking at first, but the XRF showed that only the
fingers had the thick gold, between 40-50 microinches, while the non-finger
areas had between 6-10.5 microinches.
Steve
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Thayer, Wayne - IIW
Sent: Friday, January 13, 2012 11:34 AM
To: [log in to unmask]
Subject: Re: [TN] Strange Gold? (Analysis Done!)
I agree, very nice job!
But it seems like it doesn't explicitly state the conclusion, which is (I
presume):
Someone screwed up and had the connector gold (thick) put on some of the
component mounting pads. The only way to get reliable solder joints is to
thoroughly wet it by hand and wick it off or just get new boards made
correctly.
Or am I missing something?
Wayne Thayer
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: Friday, January 13, 2012 9:27 AM
To: [log in to unmask]
Subject: Re: [TN] Strange Gold? (Analysis Done!)
I think this is an excellent report. Very interesting to see the gold
"pushed" in front of the molten solder, concentrating it. George and Andy
are to be congratulated.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Friday, January 13, 2012 7:56 AM
To: [log in to unmask]
Subject: Re: [TN] Strange Gold? (Analysis Done!)
Hope this Friday 13th is going well for everyone,
Remember my post from back in November about the strange looking gold? The
one with the purple looking solder?
Well, I got that analyzed by one of our own Technetters; George Wenger. Him
and his partner Andy Giamis were able to find time in their busy schedule to
do this for me, for which I'm humbly thankful.
It's pretty interesting. Here's my original post:
..............................
Hi All,
Below is a photo of a SON8 footprint that was printed with SAC305 on a
Gold plated PCB and reflowed. I have never seen this before. Is this "purple
plague"? If it is, exactly what causes it?
http://stevezeva.homestead.com/Strange_Gold.jpg
http://stevezeva.homestead.com/Trippy_Solder.jpg
http://stevezeva.homestead.com/Trippy_Solder_Close.jpg
Steve
..............................
I printed up one of the same panels we had the purple solder on with the
same SAC305 paste and reflowed it without parts, and got the same purple
looking solder. So I sent it to George and Andy, and here's the analysis
that they did. It's really good if you ask me.
http://stevezeva.homestead.com/FSC-5178.ppt
Steve
P.S. Thanks again George and Andy!
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
This e-mail and any files transmitted with it may be proprietary and are
intended solely for the use of the individual or entity to whom they are
addressed. If you have received this e-mail in error please notify the
sender.
Please note that any views or opinions presented in this e-mail are solely
those of the author and do not necessarily represent those of Exelis Inc.
The recipient should check this e-mail and any attachments for the presence
of viruses. Exelis Inc. accepts no liability for any damage caused by any
virus transmitted by this e-mail.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|