Hi folks -- one more comment to add to Richard's good information is that
the center pad on a QFN is the primary feature for controlling surface
tension influences for the component. If you use too much solder paste you
can cause solder joint wetting/alignment defects of the smaller outer
pads. Additionally, the amount of solder paste and the specific pattern
you use on the center pad has a large influence on how many voids you end
up with in the center pad solder joint. QFNs are a neat component
technology but have some specific assembly demands that we didn't have
before their introduction on designs.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Stadem, Richard D." <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
12/13/2011 03:01 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Stadem, Richard D." <[log in to unmask]>
To
<[log in to unmask]>
cc
Subject
Re: [TN] TI Paste Recommendations
QFNs are very typically subjected to an aperture reduction. Usually the
peripheral pads are reduced by 10-15%, and if a large belly pad is
present, the stencil aperture reduction is typically between 40% to 60% of
the pad area.
To understand why, think of it like this:
A chip capacitor, resistor, or a leaded SOIC, QFP, etc. all have someplace
for the molten solder to flow other than the pad itself. Chips have endcap
terminations, molten solder can wet out to the edges of the pads and run
up the sides of these endcap terminations. Likewise with leaded
components. In all of these cases, the solder has somewhere to go; there
is no real constraint that would cause the surface energy of the molten
solder to go "out of bounds" in the form of solder spattering.
In the case of QFNs, if you print solder paste in a one-to-one ratio with
the pads, the molten solder has no place to wet and flow. With the
component body mass sitting on the resultant puddles or blobs of molten
solder on the belly pad and the peripheral pads as well, spattering
occurs, and that is why there are so many solder fines trapped under the
QFN part. To prevent this, the stencil aperture is reduced such that the
smaller amount of solder has someplace to flow.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo
Sent: Tuesday, December 13, 2011 2:40 PM
To: [log in to unmask]
Subject: Re: [TN] TI Paste Recommendations
For QFN, 7093 is the guideline you want. QFN is rather different compare
to the BGAs.
Joyce Koo
Materials Researcher - Materials Interconnect Lab
Research In Motion Limited
Office: (519) 888-7465 79945
Mobile: (226) 220-4760
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Gerald Bogert
Sent: Tuesday, December 13, 2011 3:28 PM
To: [log in to unmask]
Subject: Re: [TN] TI Paste Recommendations
December 13, 2011
Solder paste size can depend on the part manufacturer recommendations. For
example, Freescale for their BGA P013 processor recommends that the PC
board solder pad and stencil aperture diameters should generally be the
same; a 1 to 1 ratio.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of William Noel
Sent: Tuesday, December 13, 2011 2:52 PM
To: [log in to unmask]
Subject: [TN] TI Paste Recommendations
Hello all - I am working on creating a 24 pin QFN footprint for my CAD
library. Is there a valid reason for making the solder paste smaller than
the actual pad outline? I notice that TI consistently seems to recommend
a smaller paste outline than pad outline. Additionally, they recommend a
series of small square paste squares to appear on the thermal pad rather
than a single smaller square of paste. Essentially, IPC-7351
recommendations are different than the TI recommendations. Any help?
Thank you.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the posts:
send e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives For additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute non-public
information. Any use of this information by anyone other than the intended
recipient is prohibited. If you have received this transmission in error,
please immediately reply to the sender and delete this information from
your system. Use, dissemination, distribution, or reproduction of this
transmission by unintended recipients is not authorized and may be
unlawful.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|