Hi folks - the Barney Boards were due to over cleaning which selectively
etched the tin out of the solder surface leaving it lead rich thus making
in optically "purple". As Steve McCracken detailed, you could have a
similar optical phenomena happening here with the gold/tin system. Over
cleaning isn't necessary as just simple oxidation of IMCs or the solder
joint surface or the resulting gold/tin/nickel combination may be the root
cause. As others have suggested, some SEM work to identify what elements
are present would be useful. And as a metallurgical engineer - those are
really cool looking pictures!
Dave
"Stadem, Richard D." <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
11/17/2011 02:59 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Stadem, Richard D." <[log in to unmask]>
To
<[log in to unmask]>
cc
Subject
Re: [TN] Strange Gold?
Here is some info from Hillman regarding Barney Boards like yours, Steve.
More info is in the archives simply by searching "purple solder joints".
It can be caused not just by overcleaning, but by cleaning with a somewhat
alkaline surfactant as well.
From: "Gumpert, Ben" <[log in to unmask]>
Subject: Re: Blue solder joints
X-To: TechNet E-Mail Forum <[log in to unmask]>
To: [log in to unmask]
Subject: EXTERNAL: Re: [TN] Blue solder joints
is over cleaned (say, like 10 exposures!), you actually produce a lead
(Pb) rich solder joint surface with has a "blue/purple' optical effect in
contrast to a normal solder joint which is tin rich. We used SERA analysis
a few years ago to demonstrate this effect. Doug and I have also published
the information in a couple of ppts at conferences - we call such pwas
"Barney Boards" (Barney, as in the purple dinosaur on children's
television). The optical effect is completely cosmetic and can be
eliminated by reflow the solder joints.
Subject
Re: [TN] Blue solder joints
> I seem to remember this coming up previously, but I couldn't find it in
the archives... What causes solder joints to have a blue tint?
>
> I have a card where most of the solder joints across the assembly have a
blue tint to them. It's Sn63Pb37 solder on a SnPb HASL board and a variety
of part finishes - but the pads that weren't pasted don't exhibit the blue
--------------------------------------------------------------------------------
Item #115414 (15 Aug 2011 14:26) - Re: Blue solder joints
From: "David D. Hillman" <[log in to unmask]>
Subject: Re: Blue solder joints
X-To: TechNet E-Mail Forum <[log in to unmask]>,
is over cleaned (say, like 10 exposures!), you actually produce a lead
(Pb) rich solder joint surface with has a "blue/purple' optical effect in
contrast to a normal solder joint which is tin rich. We used SERA analysis
a few years ago to demonstrate this effect. Doug and I have also published
the information in a couple of ppts at conferences - we call such pwas
"Barney Boards" (Barney, as in the purple dinosaur on children's
television). The optical effect is completely cosmetic and can be
eliminated by reflow the solder joints.
Subject
Re: [TN] Blue solder joints
> I seem to remember this coming up previously, but I couldn't find it in
the archives... What causes solder joints to have a blue tint?
>
> I have a card where most of the solder joints across the assembly have a
blue tint to them. It's Sn63Pb37 solder on a SnPb HASL board and a variety
of part finishes - but the pads that weren't pasted don't exhibit the blue
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Phil Bavaro
Sent: Thursday, November 17, 2011 2:49 PM
To: [log in to unmask]
Subject: Re: [TN] Strange Gold?
Hi Steve,
Strange footprint as well. It appears all the leads on the left are
ground and three of the four on the right are connected to the plane
with the vias.
Anyways, isn't the picture showing that the gold turned purple due to
the heating/spread of the flux? I almost have to ask if there wasn't
something wrong with the solderpaste.
Like the others have said, how many places on the board did this happen?
Was the part removed in order to take this photo?
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Thursday, November 17, 2011 10:59 AM
To: [log in to unmask]
Subject: [TN] Strange Gold?
Hi All,
Below is a photo of a SON8 footprint that was printed with SAC305 on a
gold
plated PCB and reflowed. I have never seen this before. Is this "purple
plague"? If it is, exactly what causes it?
http://stevezeva.homestead.com/Strange_Gold.jpg
Steve
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud
service.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask]
or 847-615-7100 ext.2815
-----------------------------------------------------
------------------------------------------------------------------------------
This message and any attachments are solely for the use of the addressee
and may contain L-3 proprietary information that may also be defined as
USG export controlled technical data. If you are not the intended
recipient, any disclosure, use or distribution of its content is
prohibited. Please notify the sender by reply e-mail and immediately
delete this message and any attachments.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|