Ioan,
You have gotten a lot of good answers to the question so far and I will
chip in my two cents worth.
Technically, there is no such thing as an RMA flux anymore, though the
term continues in use. RMA, Rosin Mildly Activated, was a flux
terminology from the good old days of MIL-F-14256, the military flux
specification. It was cancelled in 1995 and directed people to J-STD-004,
the current predominant flux specification in the industry. The older
rosin flux formulations that were termed RMAs, translated into ROL0, ROL1,
or ROM0, depending on the flux and who you ask. RMA fluxes are still
available, though as the market shrinks for these, they are becoming more
expensive, which encourages users to transition to something more modern.
Most people still using "RMA" flux are using the 15% solids, which is
still pretty high, compared to low residue fluxes or water soluble fluxes.
Which means there is a significant amount of flux to clean off compared
to other fluxes.
Isopropyl alcohol sucks as a cleaner, at least in my opinion. People want
to use it because it is cheap, available almost everywhere, does not
impact industrial emissions much depending on where you are in the world,
and is not a health hazard, if you don't get too wrapped around the axle
over flammability. No way, no how would I ever want to clean an RMA flux
with alcohol alone. Does not work reliably.
In my experience, high solids rosin fluxes tend to be OK if you leave them
alone, or if you totally remove them. If you "kind of" remove them, you
have a great deal of problems. You remove the encapsulating effect of the
rosin (which you want), but you free up the activators to cause havoc
(which you don't want). In my view, you want a really effective heated
saponifier in an in-line aqueous cleaner, with a thorough heated deionized
water rinse.
Doug Pauls
Ioan Tempea <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
10/28/2011 08:07 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Ioan Tempea <[log in to unmask]>
To
<[log in to unmask]>
cc
Subject
[TN] Rookie question on RMA fluxes
Dear Technos,
Although I've been around in this trade of ours for quite a while now, I
have never had the occasion to work with RMA fluxes. I need to know how
this functions. How can RMA be cleaned, I've heard about alcohol...? Is
regular aqueous wash enough? If alcohol only, do we need a special
equipment? Anything else to know?
And, anyways, are RMA fluxes still available?
Also, I imagine most of you at ease with RMA have tried to talk your
customers into converting to water soluble flux chemistries. How hard was
that? Is it possible?
Thanks,
Ioan Tempea, ing.
Ingénieur Principal de Fabrication / Senior Manufacturing Engineer
T | 450.967.7100 ext.244
E | [log in to unmask] <mailto:[log in to unmask]>
W | www.digico.cc <http://www.digico.cc/>
N'imprimer que si nécessaire - Print only if you must
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|