Hi, Jack.
If the creep corrosion is on soldermask defined pads (which it nearly always is), it is usually because the plating is applied after the masking is applied, for immersion silver plated PWBs.
This means that there is a small amount of solder mask up and over the periphery of the vias and test pads prior to the immersion silver plating. This soldermask prevents the periphery and the sides of the pads from being plated, and leaves exposed copper under the maskant.
Later, when processing the PWB through assembly cycles, some DI water mixed with small amounts of flux can become entrapped under this soldermask. A combination of water, flux, and leftover halides/bromides from the fabrication process are trapped around the exposed copper, which starts the corrosion. It usually spreads right over the top of the plated pad, and when you scrape it away you can see the nicely plated pad underneath.
Immersion silver finishes (at least the "good ones") are applied with a co-inhibitor that usually will resist any corrosion growth. However, if none of the plating is actually applied over the exposed copper on the sides of the pads, they can't do their job. The fix is to use non-soldermask defined pads if possible.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Jack Olson
Sent: Monday, July 11, 2011 9:18 AM
To: [log in to unmask]
Subject: Re: [TN] Leaded or non
I would have said that too, until I started seeing pictures of the creeping crud growth on ImAg vias in older assemblies.
(which we use for test points, so they are exposed) How do you get around that? Do you paste screen your vias? or conformal coat by default after ICT?
Jack
On Thu, 7 Jul 2011 14:26:16 -0500, David D. Hillman <[log in to unmask]> wrote:
>Hi Steve - my vote would be the ImAg and lead-free assembly choice. All
>three of your options should work with each having both pluses and
>minuses. My preference is to solder to copper rather than nickel if given
>a choice.
>
>Dave Hillman
>Rockwell Collins
>[log in to unmask]
>
>
>
>Steven Kelly <[log in to unmask]>
>Sent by: TechNet <[log in to unmask]>
>07/07/2011 12:56 PM
>Please respond to
>TechNet E-Mail Forum <[log in to unmask]>; Please respond to
>Steven Kelly <[log in to unmask]>
>
>
>To
><[log in to unmask]>
>cc
>
>Subject
>[TN] Leaded or non
>
>
>
>
>
>
>Hi All,
>I have an 18 layer rigid flex (buried and blind) that we are preparing to
>put the surface finish on and then assemble.
>Lots of BGA's etc.
>The BGA's are lead free.
>Options:
>
>1) ENIG and lead free assembly
>
>2) Immersion silver and lead free assembly
>
>3) HASL and leaded assembly
>Hi end military product.
>
>Thoughts or comments would be appreciated.
>Thanks. Steve Kelly
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 16.0
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>For additional information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
>
>
>
>______________________________________________________________________
>This email has been scanned by the MessageLabs Email Security System.
>For more information please contact helpdesk at x2960 or [log in to unmask]
>______________________________________________________________________
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 16.0
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
>-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|