Dave!
I agree with everything you stated. I typically use only two tacky fluxes, and a special heated spray application onto the PWB. I forgot to mention the dipping method. I even went so far as to set up a heated valve on my client's Mydata machines that uses a small heater to bring the tacky flux up to a whopping 100 degrees Fahrenheit (the point at which the tacky flux or the proprietary oxygen evacuation fluids become liquid) and then it uses a mild ultrasonic burst timed by the machine. This US burst of "liquid tacky flux" or OEF fluid provides an ideal coating of flux for small flip chips, CSPs, etc. By the time the component travels from the spray head to the pads on the target board, it has reverted to a tacky paste or liquid coating.
But because of the voiding inducement and the other issues, I still prefer not using paste whenever possible. Just because something is not specifically listed in IPC 7711 does not mean it is verboten.
For example, we routinely use custom laser machines at Analog Technologies for ball attach methods as well as for stripping off the old balls. These are proprietary, patented methods and materials, fully qualified for our military and space customers, and will never appear in detail in IPC 7711, or any other specification for that matter.
And I agree voids are not the end of the world. But I still don't like them, and the data supports that feeling. I look forward to Rockwell's release.
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Thursday, July 07, 2011 11:10 AM
To: TechNet E-Mail Forum; Stadem, Richard D.
Cc: [log in to unmask]
Subject: Re: [TN] BGA Repair Methods
Hi Richard! Good discussion. I agree that there is no loss of solder joint integrity with a tacky flux only BGA repair. But using a solder paste does have some advantages in terms of potential component coplanarity issues and a solder paste repair tends to be cleaner than a tacky flux only repair (dependant on the flux type and cleaning methodology). Doug and I presented a paper at the 2010 IPC APEX Conference discussing the use of "dippable" solder paste as a third alternative for BGA repair (paper title: "Investigation of Process Feasibility / Compatibility and Solder Joint Reliability of Tin-Lead Dippable Solder Paste Ball Grid Array (BGA) Component Rework/Repair"). The dippable paste option has many of the advantages of both the standard solder paste and the tacky flux only methods. The -55C to +125C thermal cycle testing showed no difference in solder joint integrity for the BGA component tested. As for the second topic of BGA voids, I would agree that a non-voided BGA solder joint is what we should be creating but having voids isn't the end of the world. Rockwell Collins and Nordson Dage are presenting a paper titled "The Last Will and Testament of the BGA Void" at the October SMTAI Conference in Fort Worth. The data set demonstrates the influence on a void on the solder joint integrity of a BGA is not as strong as some schools of thought believe. Rockwell Collins is also going to propose revised BGA void criteria to the JSTD-001 committee based on the testing so everyone should be able to get a copy of the data later this fall for review.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Stadem, Richard D." <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
07/07/2011 09:00 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Stadem, Richard D." <[log in to unmask]>
To
<[log in to unmask]>
cc
Subject
Re: [TN] BGA Repair Methods
While a crack can propagate through a BGA solder joint due to delta CTEs between the BGA substrate and the board substrate, some look at the void as a stress relief valve where the crack stops, and thus assume that because the remaining SJ hangs on awhile longer there is an improvement in reliability.
However, my feeling is that if there was no voiding in the first place, the amount of overall flexural stresses seen on the collective BGA solder joints in the first place would be less.
I learned this when performing life-cycle testing on solder pastes. When I soldered several BGAs to a test board using a solder paste with a known propensity for inducing voids (and the voids were carefully located and marked ahead of time with X-ray images), the overall time to failure where any one of the solder joints would fail electrically was much less than the test board where all of the BGAs were soldered with a paste that had very little or no voids at all.
The amount of grain coarsening after 50, 100, 500, and 1000 cycles was less on the boards with no BGA voids than was seen on the microsections of the boards with BGA voids, even though both sets of boards went through the same life-cycle testing, at the same time and in the same chamber.
But the NON-BGA component microsections did not show the exact same results. The leaded components were the same, with a small amount of variation in the chip caps/resistors.
-----Original Message-----
From: Amol Kane [mailto:[log in to unmask]]
Sent: Thursday, July 07, 2011 7:39 AM
To: TechNet E-Mail Forum; Stadem, Richard D.
Subject: RE: [TN] BGA Repair Methods
Richard! Great e-mail compiling all the reasons. We do flux only rework and I have a standard document I send our customers outlining the reasons if they question the process. Some of your points are definitely going into it! :-)
One item about voids however piqued my curiosity. You say " More voids in the BGA solder joints. Solder paste is known to induce voiding in BGAs. Never mind what they say about BGA solder joints with voids not being a reliability issue; they are."
Why do you say that?.....can you share any literature/insights/experiences that led to this opinion?
Thanks!
Amol Kane | Process Engineer
Catalyst Manufacturing Services, Inc.
941 Route 38, Owego NY 13827
Phone: (607) 687-7669 Extn 349 | Website: www.catalystems.com
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: Wednesday, July 06, 2011 11:59 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Repair Methods
I am sorry, Russ, but your EMS suppliers are right.
Additional volume of solder does NOT, and I repeat, does NOT increase BGA solder joint reliability for BGAs whose balls are intended to collapse during reflow (those with Sn63 and SAC alloy balls, but not Pb90). A larger cheese loaf is just that, a larger cheese loaf. It does not increase the modulus of elasticity.
The use of paste typically only increases the overall volume of solder about 1% or 2%, anyway. There is no real reliability difference in a solder ball that is .030" in diameter as opposed to one that is .031" in diameter, provided both are fully wetted on the pads.
IPC 7095 states:
"7.1.1.3 Importance of Paste Volume
For plastic BGAs much of their solder volume is supplied by the solder ball
on the part itself and the paste volume is not all that critical.
For BGAs above 0.80 mm pitch, stencil thickness will
be dictated by the other component types used on the
printed board assembly. Solder volume and stencil thickness
become more critical for ceramic and fine-pitch BGA
such as CSP. The solder balls used on ceramic BGAs are
not eutectic and do not collapse during the reflow process
(see Figure 7-1).
Because the high lead content ball does not collapse having
sufficient solder paste is critical. The fillet between the
land and ball depend upon the solder paste volume.
Ceramic BGA requires a minimum of 0.08 cubic mm and
a nominal 0.12 cubic mm paste volume."
Therefore, a requirement that solder paste be used for standard BGA rework is only going to lead to the following:
1. More Head-in-pillow solder joints caused by marginal reflow profiles, where the paste and the ball do not both go into liquidus.
2. More voids in the BGA solder joints. Solder paste is known to induce voiding in BGAs. Never mind what they say about BGA solder joints with voids not being a reliability issue; they are.
3. More non-agglomerated (renegade) solder fines and particles. It is difficult to manually screen paste and get it all on the pad.
4. More solder bridges caused by excessive or smeared paste prints, leading to additional subsequent reworks.
5. More flux residue. The flux in reflowed solder paste is much harder to clean than the tacky flux designed for rework.
6. Much more cost, from a rework standpoint. Applying a thin veneer of tacky flux on the board pads as opposed to carefully aligning a metal microstencil or stick-on stencil and printing paste is much less time consuming.
Solder paste is printed prior to BGA placement only because it is a convenient method of applying flux to the BGA pads during original SMT assembly. The additional metal volume (from the solder paste) is absolutely not needed.
If you are really concerned about BGA ball joint reliability, then increase the modulus of elasticity by providing solder columns rather than cheese loafs. This concept was explained in Werner Engelmaier's article awhile back, which included an outline of my cornerbonding process and my pictures of cornerbonded BGAs with solder columns rather than cheese loaves. Once this is done, the BGA typically ran several thousand more cycles before failure. The solder columns are not "added", they are created using the solder balls that come with the BGA.
I have reworked hundreds of thousands of BGAs without using paste, for many companies. None have shown any difference in reliability than BGAs either reflowed with paste as part of the original process, or reworked with paste. In fact, I have data that shows a reworked BGA using only tacky flux is more reliable. Why? Because a reworked BGA will have the benefit of pre-tinned pads with tacky flux applied, without any of number 1-6 above.
One final note: There should be little or no no-clean tacky flux seen after rework. A very thin "veneer" of a good tacky flux applied to the board pads is all that is required. I prefer water soluble tacky fluxes, and I am not afraid to state the Alpha WS 619 is an excellent halide-free tacky flux to use, with excellent cleanability in water.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Russ
Sent: Tuesday, July 05, 2011 10:15 AM
To: [log in to unmask]
Subject: [TN] BGA Repair Methods
Hello TechNetters,
I have a question about acceptable BGA repair methods. I have always required my EMS's to pre-apply solder paste to either the PWB or device prior to placing and reflowing a BGA. Some of my EMS's pushed back initially but always complied. IPC-7711/21B has two defined repair methods which both require adding solder by either pre-applying solder by using solder wire (section 5.7.1) or using solder paste (Section 5.7.2). No where does IPC-7711/21B state that you can get by with only applying tacky flux. Here is where I feel there is a conflict. In IPC-7095B Section 6.1.2 it states a couple places that you must "new solder paste or flux". No where does it mention pre-applying wire solder before applying the flux. IPC may want to review the wording there.
I am not sure how you would control manually applying core (wire) solder so I only consider pre-applying solder paste an acceptable method. I am a firm believer that by not applying solder paste reduces the solder volume, joint height and thereby reducing reliability of the solder joint.
First, I would like to know if anyone knows of a published reliability study of Flux only versus Pre-pasting a BGA repair.
Second, I would like to hear other opinions on this subject.
From a processing standpoint I understand the EMS's position that applying tacky flux makes the BGA repair a whole lot easier and cheaper as adding paste requires a mini-stencil and a trained operator. I am all for easy if it does not but reliability at risk. I also have a concern about the excessive flux that I find under a BGA that has been attached with only tacky flux. They are no-clean fluxes but but excess is never good or pretty. Thanks in advance.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|