Hi Chris - sorry for the slow response. Part of the answer for the
difference in solder joint heel fillet requirements is the lead geometry.
An "L" shape has less compliancy than the "J" shape so having additional
solder provides some additional solder joint integrity life. In many
product use environments, we would be hard pressed to demonstrate a
statistical difference in solder joint integrity for the two
configurations and in many cases, even if there was a statistical
difference, the practical difference may be zero. However, the JSTD-001
committee has used past/present solder joint integrity data to establish
the current solder joint fillet requirements for the whole of the
industry. The requirements can be revised if new data/test results are
submitted to the committee supporting a change in the requirements. You
can use the IPC SM 785 specification to calculate a first order difference
estimate. Hope this helps.
Dave
Chris Mahanna <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
06/22/2011 03:50 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Chris Mahanna <[log in to unmask]>
To
<[log in to unmask]>
cc
Subject
Re: [TN] Min fillet height gull/J vs. L
Yes. Although I suppose 7.5.9 vs. 7.5.13 is a better example in that both
are inward formed.
Chris
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Wednesday, June 22, 2011 4:28 PM
To: TechNet E-Mail Forum; Chris Mahanna
Cc: [log in to unmask]
Subject: Re: [TN] Min fillet height gull/J vs. L
Hi Chris - for clarity reasons, which figures in IPC JSTD 001 are you
comparing? Section 7.5.7 vs 7.5.13?
Dave Hillman
Rockwell Collins
[log in to unmask]<mailto:[log in to unmask]>
Chris Mahanna <[log in to unmask]<mailto:[log in to unmask]>>
Sent by: TechNet <[log in to unmask]<mailto:[log in to unmask]>>
06/22/2011 03:20 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]<mailto:[log in to unmask]>>; Please
respond to
Chris Mahanna <[log in to unmask]<mailto:[log in to unmask]>>
To
<[log in to unmask]<mailto:[log in to unmask]>>
cc
Subject
[TN] Min fillet height gull/J vs. L
Hello all, can someone tell me-
What is it that necessitates the ~25% H additional height to a L-lead
fillet when compared to J or gull?
My guess would be diff. CTE and J, Gull have some relief, but I need more
than a guesstimate.
Thanks in advance,
Chris
Chris Mahanna
Robisan Laboratory Inc.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]<
mailto:[log in to unmask]>
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask]<mailto:[log in to unmask]
> with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask]<
mailto:[log in to unmask]> or 847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|