Technetters,
We have confirmed that a returned product from the field has failed die
to silver sulfide contamination.
The conclusion from the analysis is:
Based on the analysis performed, the "black" contaminant material is
silver sulfide, a common silver corrosion product. This corrosion often
occurs when silver plating is exposed to atmospheric pollution that
contains high levels of sulfur compounds (exhaust from fossil fuels).
We have confirmed that in particular resistor networks are susceptible
due to the silver content that apparently is exposed on the top of the
component. We have not observed issues with any other component types.
The obvious answer to how to protect a product in this environment is to
use conformal coating. However, from what I have read there are only
very few coating materials that can actually protect from silver sulfide
corrosion. Epoxy based conformal coatings is the only ones that will
successfully pass ASTM N 809 test. My question to the experts is if
there are other solutions or coatings you have been successful with or
if someone has actually solved this issue in different ways. It seems
this should be an important issue for the automotive electronics industry.
Some one suggested using solder to cover the component, but I can not
understand how that could work.
As always, thank you for your insight.
--
Leif Erik Laerum
CONFIDENTIALITY NOTICE: This email and any attachments are Texas Memory Systems' proprietary material for the exclusive and confidential use of the intended recipient. If you are not the intended recipient, please do not read, distribute or take action in reliance upon this message. Any unauthorized disclosure is prohibited. If you have received this in error, please notify us immediately by return email and promptly delete all copies of this message and its attachments from your computer system.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|