Hi Louis - yes, as a generalized answer, you will reach a constant value
provided you are: (1) de-drossing on a regular basis and removing a
consistent volume; (2) the quantities of assemblies and their surface
finish is relatively constant; (3) the wave solder pot temperature and
conveyor speed are relatively constant. Reaching a constant level of any
element in the solder pot is a balance of what goes thru the wave solder
pot and what gets removed in the de-drossing step. We run very little OSP
boards so the copper levels don't move around much on our solder pot. We
do run a bunch of ENIG and ImAg boards which ends up coming out in the
dross provided our volumes stay consistent. You can get some copper to
come out in the dross but if you are running a heavy volume of OSP boards,
you might have to take measures to balance copper content. The only time
we have ever had an element compliance issue was with a mini-wave
solderpot when we processed a serious volume of gold plated connectors
which spiked to gold content of the solder pot out of compliance. I have
been fortunate to never have to drain a solder pot due to a element
compliance issue.
Dave
Louis Hart <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
03/11/2011 10:06 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Louis Hart <[log in to unmask]>
To
[log in to unmask]
cc
Subject
Re: [TN] Solder bath analysis. Sn63Pb37 alloy.
Dave et al, let me ask a question about solder pot maintenance about which
I've been curious for a long time.
If the dross is skimmed off the top of a pot (that is being used for
soldering or for HASL), will the copper concentration eventually reach
some (within the limits of measurement error)constant value? My theory is
that it will.
Louis Hart
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of David D. Hillman
Sent: Friday, March 11, 2011 9:31 AM
To: [log in to unmask]
Subject: Re: [TN] Solder bath analysis. Sn63Pb37 alloy.
Hi folks! In the IPC-HDBK-001 Handbook, section 5.3.7, page 62 is the
formula you can use for calculating how much tin you add to the wave
solder pot for tin replenishment efforts.
Dave Hillman
Rockwell Collins
[log in to unmask]
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|