Cedric,
Richard and Paul are correct that the violates is solder paste are the root cause for voiding especially when the RF transistor is in a recessed cavity. The violates have no where to go.
I think you have two choices. You can pre-tin both surfaces with lots of solder and then reflow with a very thin sheen of flux as Richard suggests or you can place a solid preform coated with a very thin layer of a non-clean LSF in the cavity before placing the RF transistor and then reflow. The real trick is to apply as little flux as possible.
Regards,
George
George M. Wenger
Senior Principal Reliability / FMA Engineer
Andrew Corporation - Wireless Network Solutions
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 Office (732) 309-8964 Mobile
E-mail: [log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Cedric ORAIN
Sent: Thursday, February 17, 2011 2:53 PM
To: [log in to unmask]
Subject: Re: [TN] Voids issue on Aluminium base plate
George,
It is in a recessed cavity.
Regards,
Cedric
-----Message d'origine-----
De : TechNet [mailto:[log in to unmask]] De la part de Wenger, George M.
Envoyé : jeudi 17 février 2011 17:48
À : [log in to unmask]
Objet : Re: [TN] Voids issue on Aluminium base plate
Cedric,
What is the size of the RF transistor base? Is the transistor on a flat
aluminum surface or is it in a recessed cavity on an aluminum chassis?
Regards,
George
George M. Wenger
Senior Principal Reliability / FMA Engineer
Andrew Corporation - Wireless Network Solutions
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 Office (732) 309-8964 Mobile
E-mail: [log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Phil Bavaro
Sent: Thursday, February 17, 2011 11:27 AM
To: [log in to unmask]
Subject: Re: [TN] Voids issue on Aluminium base plate
Cedric,
Lots of things come to mind....plating thicknesses, paste patterns,
wetting, profiles.
Is there any pattern to the voiding? Does it resemble the printed paste
shape?
I have soldered lots of RF transistor bases down, but I haven't ever
soldered them to NiAg plated aluminum (always to Ni/Au plated copper
slugs).
You don't mention the paste patterns used but that will contribute to
large voiding if you don't give the gases a path to get out. I would
reduce the solder paste coverage to 45%, use a checkerboard pattern of
dots, and then observe the voiding pattern.
This assumes that the voiding is not relative to wetting as that will
change everything. To do this, check the solderability of both surfaces
being soldered to independently.
Phil
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Cedric ORAIN
Sent: Thursday, February 17, 2011 6:26 AM
To: [log in to unmask]
Subject: [TN] Voids issue on Aluminium base plate
Dear Technetters,
We have to solder a RF power transistor onto an aluminium base plate and
we
are facing with a very challenging issue.
We encountered a high voids rate (>30% or 40%) underneath the component
body
(which is about 35x10mm). This is not acceptable for this application.
The component is Nickel/gold plated whereas the aluminium baseplate is
plated with Nickel and Silver and then cleaned with solvent.
We tried to change/adapt:
- soak time of the profile,
- 2 difference solder pastes (SAC305),
- change the screen design and thickness
Finally none of these parameters looks to have significant effect on
voids
rate. We are now wondering if the solderability of the Ni/Ag plating is
good
enough and even if it is convenient for that purpose.
Is somebody could give us advises? How to enhanced NiAg plating
solderability (acid ?!, ...)? Which flux could help to compensate the
poor
wettability? Which kind of plating would be preferable? ...
Thanks and regards,
Cedric
----------------------------------------------------------------------------
--
This message and any attachments are solely for the use of the addressee and
may contain L-3 proprietary information that may also be defined as USG
export controlled technical data. If you are not the intended recipient, any
disclosure, use or distribution of its content is prohibited. Please notify
the sender by reply e-mail and immediately delete this message and any
attachments.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|