Leland,
You might want to look at the ball to BGA side of the joint...
Normally the BGA substrates are finished with Ni-Au...
If HiP is ruled out and flexure gives operation then I would look there...
Unless you have bulk solder failure at the interface between the balls and the PCB it can be difficult to get enough pressure over a enough balls to force them to collapse enough to make contact...
I am assuming that the BGA in question has an epoxy over-mold that does not completely cover the BGA substrate and that you are not using solder-mask defined pads on the failing pads....
Paul
Paul Edwards
Surface Art Engineering
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall
Sent: Thursday, December 02, 2010 10:24 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Failure Analysis Recommendations
Jerry,
They successfully demonstrated detection of opens, ball separations, and
head in pillow conditions when we qualified our machine prior to the
purchase. That's why we're all scratching our heads over this
particular failure...
Leland
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Jerry Dengler
Sent: Thursday, December 02, 2010 1:18 PM
To: [log in to unmask]
Subject: Re: [TN] BGA Failure Analysis Recommendations
Hi Leland,
Maybe you can talk to the X-ray manufacturer to see if they can come in
and show you how wonderful their machine really is by finding this
fault.
Jerry
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall
Sent: Thursday, December 02, 2010 1:04 PM
To: [log in to unmask]
Subject: Re: [TN] BGA Failure Analysis Recommendations
Maybe our 3D X-ray needs a little tweaking in some form or fashion.
We've yet to utilize it a lot for failure analysis (because, thank
heavens, this is the first we've had).
Leland
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of vladimir Igoshev
Sent: Thursday, December 02, 2010 12:48 PM
To: [log in to unmask]
Subject: Re: [TN] BGA Failure Analysis Recommendations
And that was exactly why I said that good (high resolution) X-ray
inspection should be done first :-)
Vladimir
SENTEC Testing Laboratory Inc.
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
-----Original Message-----
From: "Wenger, George M." <[log in to unmask]>
Sender: TechNet <[log in to unmask]>
Date: Thu, 2 Dec 2010 11:41:01
To: <[log in to unmask]>
Reply-To: TechNet E-Mail Forum <[log in to unmask]>,
"Wenger, George M." <[log in to unmask]>
Subject: Re: [TN] BGA Failure Analysis Recommendations
Leland,
I don't usually make guesses but if I had to guess I think you might
have a case of Head-in-Pillow.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M.
Sent: Thursday, December 02, 2010 12:00 PM
To: [log in to unmask]
Subject: Re: [TN] BGA Failure Analysis Recommendations
Vladdimir you are correct but it is not as likely as ENIG
Regards,
George
George M. Wenger
Senior Principal Reliability / FMA Engineer
Andrew Corporation - Wireless Network Solutions
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 Office (732) 309-8964 Mobile
E-mail: [log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of vladimir Igoshev
Sent: Thursday, December 02, 2010 11:25 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Failure Analysis Recommendations
I thought I would mention that Brittle Fracture is not limited only to
ENIG with lead-free solders :-)
Vladimir
SENTEC Testing Laboratory Inc.
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
-----Original Message-----
From: "Wenger, George M." <[log in to unmask]>
Sender: TechNet <[log in to unmask]>
Date: Thu, 2 Dec 2010 10:10:25
To: <[log in to unmask]>
Reply-To: TechNet E-Mail Forum <[log in to unmask]>,
"Wenger, George M." <[log in to unmask]>
Subject: Re: [TN] BGA Failure Analysis Recommendations
Leland,
Since the PCB is OSP and not ENIG I would suspect a
solderability/soldering defect before a brittle interface fracture.
If you decide to do DPA cross sectioning then I would suggest cutting
the BGA out from the board close to the BGA perimeter and then looking
at each side of the BGA with a convention microscope before cutting the
BGA up for cross sectioning. Sometime you can see a couple of rows into
the BGA.
Regards,
George
George M. Wenger
Senior Principal Reliability / FMA Engineer
Andrew Corporation - Wireless Network Solutions
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 Office (732) 309-8964 Mobile
E-mail: [log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall
Sent: Thursday, December 02, 2010 11:02 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Failure Analysis Recommendations
Richard,
We've priced but not yet purchased a BGA inspection scope. I'll check
the one you've mentioned below from Practical. It might be thousands
cheaper than what we're considering, and yet perform the same function.
As far as the component, it was not reworked. The unit passed all our
in-house testing before being submitted to our HALT process.
The board finish is OSP.
Leland
-----Original Message-----
From: Stadem, Richard D. [mailto:[log in to unmask]]
Sent: Thursday, December 02, 2010 10:57 AM
To: TechNet E-Mail Forum; Leland Woodall
Subject: RE: BGA Failure Analysis Recommendations
Or you have an internal via barrel crack.
One way to tell is to purchase the small inspection prisms from
Practical Components. No BGA assembler/inspector should be without one.
You can use any standard microscope and the inspection mirror to see
under almost any BGA. The prism has a beveled edge so you can get right
down to the PWB, and you can angle the mirror to obtain the best view.
The prism is mounted on the end of a small wire that goes into a handle
much like an exacto knife handle. Imagine a 9-iron with a highly
polished face, but in miniature. To use it, you only need about .070"
clearance around the BGA periphery.
Back to the cause of the intermittent open.
If the BGA was previously reworked, and this did not fix the issue, then
it is probably an internal via separation. These are quite often
mistaken for a bad BGA solder connection. If it is a solder joint issue,
it is usually either BP or BF.
What is the circuit board finish?
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall
Sent: Thursday, December 02, 2010 9:36 AM
To: [log in to unmask]
Subject: [TN] BGA Failure Analysis Recommendations
Good morning, everyone!
I'm looking for some advice on how to best analyze a BGA problem. We
had an assembly to fail in a reliability test, and have isolated the
problem to an intermittent contact on the BGA device. When downward
pressure is applied to the component it will pass. Without the
pressure, it won't.
That tells me we have either fractured a joint, had a ball to separate
from the package, or had a head in pillow (or non-wet) condition.
We don't have a BGA inspection scope in house, and I can only see two of
the four outside edges with the equipment I have. Of course, nothing is
wrong with those.
We have both 2 and 3D xray machines, but neither detect a flawed
condition.
At this point, do I go with dye and pry, or conduct a series of cross
sections?
What's the recommendations of the pros out there that have dealt with
this? Your suggestions are sincerely appreciated!
Leland Woodall
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
==============================================================================
This email and any attachments thereto may contain private, confidential, and
privileged material for the sole use of the intended recipient. Any review, copying,
or distribution of this email (or any attachments thereto) by others is strictly prohibited.
If you are not the intended recipient, please contact [log in to unmask]
immediately and permanently delete the original and any copies of this email and
any attachments thereto.
==============================================================================
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|