TECHNET Archives

December 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Leland Woodall <[log in to unmask]>
Date:
Thu, 2 Dec 2010 10:02:36 -0600
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Wenger, George M." <[log in to unmask]>
Subject:
From:
"Wenger, George M." <[log in to unmask]>
MIME-Version:
1.0
In-Reply-To:
Content-Transfer-Encoding:
8BIT
Content-Type:
text/plain; charset="us-ascii"
Parts/Attachments:
text/plain (80 lines)
Leland,

I think there are many on TN that can give you recommendations but before they do they probably will have several questions for you.
My questions would be:
1. What is the PCB surface finish?  Is it ENIG?
2. What is the pitch of the BGA and how large (# of I/O) is the BGA?
3. When you say you've isolated the problem to an intermittent BGA contact, have you isolated the intermittent to a particular ball or location on the BGA?  Is the intermittent at the corners or on outer rows or near the perimeter?
4. When you say X-Ray didn't detect a flaw how close (what magnification did you look at the BGA balls) did you examine the BGA?  Did you look at the over all BGA or go ball by ball?  If you went ball by ball and were able to see evidence of solder paste filleting on all balls that it probably wasn't a plugged stencil but may be a fractured solder joint.

Regards,
George
George M. Wenger
Senior Principal Reliability / FMA Engineer
Andrew Corporation - Wireless Network Solutions
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 Office (732) 309-8964 Mobile
E-mail: [log in to unmask]

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leland Woodall
Sent: Thursday, December 02, 2010 10:36 AM
To: [log in to unmask]
Subject: [TN] BGA Failure Analysis Recommendations

Good morning, everyone!

I'm looking for some advice on how to best analyze a BGA problem.  We
had an assembly to fail in a reliability test, and have isolated the
problem to an intermittent contact on the BGA device.  When downward
pressure is applied to the component it will pass.  Without the
pressure, it won't.

That tells me we have either fractured a joint, had a ball to separate
from the package, or had a head in pillow (or non-wet) condition.

We don't have a BGA inspection scope in house, and I can only see two of
the four outside edges with the equipment I have.  Of course, nothing is
wrong with those.

We have both 2 and 3D xray machines, but neither detect a flawed
condition.

At this point, do I go with dye and pry, or conduct a series of cross
sections?

What's the recommendations of the pros out there that have dealt with
this?  Your suggestions are sincerely appreciated!

Leland Woodall

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2