TECHNET Archives

November 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
"David D. Hillman" <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Date:
Wed, 10 Nov 2010 07:09:14 -0600
Content-Type:
text/plain
Parts/Attachments:
text/plain (92 lines)
Hello! I recommend you conduct a solderability test in accordance with the 
IPC JSTD-003 specification. The issues you describe are root caused in the 
plating process and you can demonstrate to your ribbon manufacturer that 
the wetting is not acceptable per a consensus standard and that there is a 
need to correct the situation. Good Luck.

Dave Hillman
Rockwell Collins
[log in to unmask]




[log in to unmask] 
Sent by: TechNet <[log in to unmask]>
11/10/2010 12:58 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
[log in to unmask]


To
[log in to unmask]
cc

Subject
[TN] Question on ENIG process






Hello technetters.
We have a bad wettability (SnPb process) on some copper ribbons covered by 

a Ni layer and Au layer. These are applied by an ENIG process.
The ribbon no-wet area is located on alongside and edges of ribbons. No 
issue in the centrum area of the ribbon. The ribbons are 3 mm width and 
0.3 mm thick.
The Ni layer and Au layer have the good thickness : 4µm and 0.1 µm. But 
with a SEM analysis we see in the bad area a porous Au. 
At the degolding operation, the area becomes black, the SnPb don't  wet 
and the SEM analysis gives a high presence of Phosporus in that area 
(Qualitative analysis, the P peak is half the Ni peak).
At soldering operation more you try and worse it is.
The manufacturer of the ribbon says the P in the Ni-P bath is 9%.
Question:
I think the cause is a bad control and homogeneity of the Ni-P bath. Is it 

correct or could be another cause as "only"  2/3 of the lot is bad?
After ENIG process, how many P has to remain on the Ni layer ?
Thanks for your answers.

Best regards,
CANTAGALLO Luigi

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2