Cu-S complex. Residue etchant or other chemicals traped there. If they use UV cure mask, un cured mask may have S containing chemicals that react with Cu. Inside via is difficult to cure. Just an off shot Guess.
--------------------------
Sent using BlackBerry
----- Original Message -----
From: Steve Gregory [mailto:[log in to unmask]]
Sent: Wednesday, November 17, 2010 08:26 AM
To: [log in to unmask] <[log in to unmask]>
Subject: Re: [TN] Radially discoloration on solder-resist covered via holes, why?
Hi Colin,
The thing that confuses me, is that Charming said that the boards looked
fine after assembly, and it was only after the boards had been stored a
while did they notice the dark areas around the vias. If it was thicker mask
over the vias you should have seen that from the beginning, right?
Steve
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of colin mcvean
Sent: Tuesday, November 16, 2010 7:15 PM
To: [log in to unmask]
Subject: Re: [TN] Radially discoloration on solder-resist covered via holes,
why?
I agree with the plugged via scenario....
The possible reason for "discolouration" could be the fact that the plugging
process is a seperate screening process, using a stencil screen with only
vias open. Normal PSR is then applied over the top of semi-cured plugged
vias, and process photomechanically. This would account for a thicker
deposition at the via hol area, and also the darker contrast of colour.
Microsection of the via hole would verify the situation....
My 2p worth
--- On Tue, 16/11/10, Bob Landman <[log in to unmask]> wrote:
From: Bob Landman <[log in to unmask]>
Subject: Re: [TN] Radially discoloration on solder-resist covered via holes,
why?
To: [log in to unmask]
Date: Tuesday, 16 November, 2010, 22:48
I think you nailed it Inge. All the bad holes are plugged vias. The open
vias are very tightly registered.
Bob
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Inge
Sent: Tuesday, November 16, 2010 2:11 PM
To: [log in to unmask]
Subject: Re: [TN] Radially discoloration on solder-resist covered via holes,
why?
Had a brief look in some of our company papers about the second guess. We
observed a difference between plugged and unplugged vias. The former were
discolored like yours and it was caused by overtemperature (Leadfree!)
which degraded the epoxy which bleeded out some stuff that discolerd the
soldermask. What chemistry process, I don't remember.
Inge
----- Original Message -----
From: "Inge" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Tuesday, November 16, 2010 7:44 PM
Subject: Re: [TN] Radially discoloration on solder-resist covered via holes,
why?
> It may be what we name 'via halo' effects,which is caused by stress.
> We do not accept.
> It may also be caused by contaminations and/or improper drying.
>
> / Inge
>
>
> ----- Original Message -----
> From: "Victor Hernandez" <[log in to unmask]>
> To: <[log in to unmask]>
> Sent: Tuesday, November 16, 2010 7:22 PM
> Subject: Re: [TN] Radially discoloration on solder-resist covered via
> holes, why?
>
>
> Is there a higher mag photo of this anomaly. I need to see it, to call
> it.
>
> "X"
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Ian Hanna
> Sent: Tuesday, November 16, 2010 12:20 PM
> To: [log in to unmask]
> Subject: Re: [TN] Radially discoloration on solder-resist covered via
> holes, why?
>
> the discoloration is visible on top of the surface copper just right
> of
> R52 -- this suggests it is a surface condition of the mask or between
> the mask and the surface copper and not an internal condition
>
>
>
>
>
> Chuck Brummer <[log in to unmask]>
> Sent by: TechNet <[log in to unmask]>
> 11/16/2010 01:14 PM
> Please respond to
> TechNet E-Mail Forum <[log in to unmask]>; Please respond to
> [log in to unmask]
>
>
> To
> [log in to unmask]
> cc
>
> Subject
> Re: [TN] Radially discoloration on solder-resist covered via holes, why?
>
>
>
>
>
>
> Charming,
>
> I think you need a micro section and it will reveal bad news. Rudy
> may be
>
> right or there may be an internal separation. Is this a multi layer?
> I once saw a set of boards on which they spend to much time in the
> glass etch and when copper plating the holes the copper wicked up the
> glass fibers.
>
> Chuck Brummer l 3M Manufacturing Engineer 3m Electronic Solutions
> Division--Flexible Circuits
> 8357 Canoga Ave. l Canoga Park, CA 91304-2605
> (818) 734-4930
> [log in to unmask] l www.3m.com l www.3mFlex.com
>
>
>
>
> From:
> Steve Gregory <[log in to unmask]>
> To:
> <[log in to unmask]>
> Date:
> 11/16/2010 08:48 AM
> Subject:
> Re: [TN] Radially discoloration on solder-resist covered via holes, why?
> Sent by:
> TechNet <[log in to unmask]>
>
>
>
> Hi Charming,
>
>
>
> I have your picture posted, it's here:
>
>
>
> http://stevezeva.homestead.com/Pic1.JPG
>
>
>
> Maybe they weren't cleaned well before solder masking?
>
>
>
> Steve
>
>
>
> From: Charming Chan [mailto:[log in to unmask]]
> Sent: Tuesday, November 16, 2010 10:51 AM
> To: [log in to unmask]
> Subject: Radially discoloration on solder-resist covered via holes, why?
>
>
>
> Hi Steve,
>
> Would you help post the attached picture for me and forward this
> message to TechNet? Thanks a lot.
>
>
>
> The picture shows radially discoloration on solder-resist covered via
> holes, while, the immersion silver pads without solder-paste reflowing
> have shiny appearance with no discoloration. With naked eye checking,
> the discoloration on solder-resist covered via holes is not corrosion
> product.
>
>
>
> BTW, the pcb board surface finish is immersion silver, via holes are
> fully pluged with solder resist, and no discoloration is observed
> after pcb assembly finished. The discoloration possibly gets start in
> PCBA storaging.
>
> Best Regarads
>
> Charming Chan
>
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
> per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>
> for additional information, or contact Keach Sasamori at
> [log in to unmask] or
>
> 847-615-7100 ext.2815
> -----------------------------------------------------
>
>
>
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
> per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at
> [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
> per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at
> [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
> per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at
> [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or
> [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
> unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
> or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
> per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at:
> http://listserv.ipc.org/archives Please visit IPC web site
> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at
> [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|