TECHNET Archives

November 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Tue, 23 Nov 2010 20:51:19 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Werner Engelmaier <[log in to unmask]>
Subject:
From:
Werner Engelmaier <[log in to unmask]>
Content-Type:
text/plain; charset="utf-8"
In-Reply-To:
<9031E3D59F6E4AC69D115AE7FFCC2FF7@dell3a3601fa11>
Content-Transfer-Encoding:
quoted-printable
MIME-Version:
1.0
Parts/Attachments:
text/plain (95 lines)
 Inge,
Indeed,some of the IMCs in these figures are needle-like, but I am not at all sure they are SnAg-IMCs. They could just as well be Cu6Sn5, which has not shown to embrittle the solder structure.
Werner

 


 

 

-----Original Message-----
From: Inge <[log in to unmask]>
To: [log in to unmask]
Sent: Tue, Nov 23, 2010 6:01 pm
Subject: Re: [TN] Ductile to Brittle transition


In fig 14 and 15 you say that IMCs are sticking out , and as I can see it, they are needles. 
 
Inge 
 
 
Hi Inge, 
1. Not a good simile—the steel in concrete only adds strength in tension, not compression, it is not brittle, and it is round; IMCs are NOT needles—they only appear that way when the platelets are sectioned at acute angles; the adhesion of the concrete to steel is very high, not so solder to IMC. 
2. Crystal growth at times appears [at least] chaotic. 
3. I think it is the basic material properties—similar to all crystal structure—high modulus and little ductility. 
4. Certainly the presence of the constituent metals is required—Margareta Nylen in Sweden has shown that when all the Sn was used up in forming IMCs, no more dissolution took place—elegant experiment; solidification speed certainly would have an impact, I would think impurities as well. 
Skoal, 
Werner 
 
 
 
----- Original Message ----- From: "Inge" <[log in to unmask]> 
To: <[log in to unmask]> 
Sent: Tuesday, November 23, 2010 10:28 PM 
Subject: [TN] Ductile to Brittle transition 
 
> Hi, 
> have a few questions on Konstantina's and your report. 
> 
> 1.  If you place steel bars or steel nets in the concrete, the strength > will increase significantly, but the IMC plates and needles in the sollder > joint do the opposite. How com? 
> 
> 2. Why are so many geometries created? Large plates, small plates, > needles, bars, all in a chaotic oder. 
> 
> 3.  What causes the predominant brittleness, size of IMCs or geometric > form or  anything else? 
> 
> 4. What is the major driving force to build up the IMC structure, > percentage of xx in the solder, or solidification speed or what? 
> 
> Inge 
> 
> ______________________________________________________________________ 
> This email has been scanned by the MessageLabs Email Security System. 
> For more information please contact helpdesk at x2960 or [log in to unmask] > ______________________________________________________________________ 
> 
> --------------------------------------------------- 
> Technet Mail List provided as a service by IPC using LISTSERV 15.0 
> To unsubscribe, send a message to [log in to unmask] with following text in 
> the BODY (NOT the subject field): SIGNOFF Technet 
> To temporarily halt or (re-start) delivery of Technet send e-mail to > [log in to unmask]: SET Technet NOMAIL or (MAIL) 
> To receive ONE mailing per day of all the posts: send e-mail to > [log in to unmask]: SET Technet Digest 
> Search the archives of previous posts at: http://listserv.ipc.org/archives 
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 > for additional information, or contact Keach Sasamori at [log in to unmask] or > 847-615-7100 ext.2815 
> -----------------------------------------------------  
______________________________________________________________________ 
This email has been scanned by the MessageLabs Email Security System. 
For more information please contact helpdesk at x2960 or [log in to unmask] ______________________________________________________________________ 
 
--------------------------------------------------- 
Technet Mail List provided as a service by IPC using LISTSERV 15.0 
To unsubscribe, send a message to [log in to unmask] with following text in 
the BODY (NOT the subject field): SIGNOFF Technet 
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL) 
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest 
Search the archives of previous posts at: http://listserv.ipc.org/archives 
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815 
----------------------------------------------------- 

 

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2