Hi Chris - like all of the pwb surface finishes, immersion tin has both
advantages and disadvantages. One primary disadvantage is that immersion
tin is not very robust to oxidation degradation. Stewart detailed the
issue with oxidized IMCs which can be a big issue. SERA would be one
technique to determine what level of oxidation (both Sn and IMC) is on the
pads dependent on the BGA pad size. And yes, I would do a solderability
test after the pwbs have undergone one reflow pass - that thermal
excursion may be enough to push the immersion tin from solderable to
unsolderable. Good Luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
Chris Mahanna <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
11/23/2010 09:00 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Chris Mahanna <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] ImSn finish, BGA solderability
Due to the holiday time crunch, I'm looking for some brainstorming on ImSn
solderability forensics.
I'm thinking that there may be some low hanging fruit that I'm missing
because we just have little experience with ImSn.
We've found random one-up Pb-free BGA balls not wetted to the lands.
Finish is ImSn. Basic question in my mind is Sn oxides, SnCu
intermetallics, or misprint.
Representative bare boards passed J-STD-003 solderability with flying
colors, but it is a double sided SMT. Haven't tried after reflow
simulation yet.
Both the assemblies and representative bare boards are now naturally aged,
so SERA wouldn't quantify the problem as it existed. Would it?
I've noted the coincidence of eggshell voids with the non-wet balls.
Doesn't that imply some paste/flux? Does it imply anything else? Are the
volatiles more likely to form eggshells when they are burning through Sn
oxides?
Here are some pics:
http://ipc-technet.groupsite.com/gallery/16789
Thanks!
Chris
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|