Hi Chris,
What do you mean by 'fanout clocking?'
I think you have a combination of 'Black Pad' and component warpage.
'What points to 'Black Pad' is the periphery location—during soldering the periphery gets a lot more heat than the interior, thus more Ni goes into solution with Sn, thus leaving a higher P-concentration at periphery pads, thus they are weaker, thus component warping causes interfacial separation on the periphery & pad cratering where the P-concentration is lower.
Werner
-----Original Message-----
From: Chris Mahanna <[log in to unmask]>
To: [log in to unmask]
Sent: Mon, Oct 11, 2010 2:40 pm
Subject: Re: [TN] Mech. damage or poor wetting?
Here are a few pictures
http://ipc-technet.groupsite.com/gallery/16011
this job is a mixed bag. Currently we suspect soldering, cratering, ICT and
t-cycling damage
Chris
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Monday, October 11, 2010 2:22 PM
To: TechNet E-Mail Forum; Chris Mahanna
Cc: [log in to unmask]
Subject: Re: [TN] Mech. damage or poor wetting?
Hi Chris - do you have any pictures you can share?
Dave Hillman
Rockwell Collins
[log in to unmask]
Chris Mahanna <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
10/11/2010 11:29 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Chris Mahanna <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] Mech. damage or poor wetting?
We have a BGA dye-n-pry job that shows board side sj damage with a strong
correlation to fan-out clocking.
We also have some microsection evidence of poor wetting.
All damage/dye is on perimeters.
Is this an indication of heat sinking and subpar wetting, or can it be
completely mechanical? Both?
Thanks
Chris
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
=
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|