forgot to tell what was the reason for stopping edge coating: the UV curing
did not work well, and the conveyor band became full of sticky coatin
droplets....(did not happen to oven curing of course)
----- Original Message -----
From: "Inge" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Wednesday, October 20, 2010 10:46 PM
Subject: Re: [TN] Conformal Coating Board Edges
> Well, it depends..
>
> example 1: boards sensitive to water ingress via edges: we used
> multilayers of cc along edges
> example 2: boards with rough edges damaged the rack slides: we used cc
> along edges
> example 3: boards with smooth edges, no harsh environment: we did not use
> cc along edges
> there are more examples of course
>
> Conformal coating the edges was tricky, because of the sharp edges. The
> viscosity was therefore very important. Someone mentioned Parylene, that
> one has no such problem. Parylene is a dream stuff.
>
> Lately, we have skipped edge coating, except when the customer wants it.
>
>
> I had a look into MoonMan's POD, which covers most about PCB
> manufacturing. Strange enough, nothing about edge coating.
>
> Inge
>
> ----- Original Message -----
> From: "Douglas Pauls" <[log in to unmask]>
> To: <[log in to unmask]>
> Sent: Wednesday, October 20, 2010 8:20 PM
> Subject: [TN] Conformal Coating Board Edges
>
>
>> Good afternoon all,
>>
>> I am glad we all appreciate Inge and the time he puts into making this a
>> fun and interesting forum. To sum up: Ditto.
>>
>> I have a question related to conformal coating, a sort of survey. For
>> those of you that conformally coat your assemblies, do you coat the edges
>> of the boards? Why or why not?
>>
>> There is an internal debate here and I wanted some other viewpoints
>> before
>> offering my own.
>>
>> Doug Pauls
>> Rockwell Collins
>>
>> ______________________________________________________________________
>> This email has been scanned by the MessageLabs Email Security System.
>> For more information please contact helpdesk at x2960 or [log in to unmask]
>> ______________________________________________________________________
>>
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 15.0
>> To unsubscribe, send a message to [log in to unmask] with following text in
>> the BODY (NOT the subject field): SIGNOFF Technet
>> To temporarily halt or (re-start) delivery of Technet send e-mail to
>> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>> To receive ONE mailing per day of all the posts: send e-mail to
>> [log in to unmask]: SET Technet Digest
>> Search the archives of previous posts at:
>> http://listserv.ipc.org/archives
>> Please visit IPC web site
>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
>> information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
>> ext.2815
>> -----------------------------------------------------
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|