TECHNET Archives

September 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Glidden, Kevin" <[log in to unmask]>
Date:
Tue, 21 Sep 2010 09:28:12 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
From:
"David D. Hillman" <[log in to unmask]>
X-cc:
In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (223 lines)
Hi Kevin - both nickel/boron and nickel phosphorous plating are generally 
used as environmental/mechanical purposes such as heatsinks, rails, 
standoffs, chassis, etc. You can solder directly to them but they are not 
generally considered "electronic finishes", at least not in the same view 
as ENIG, ImAg, ImSn or HASL. You can solder directly to the EN electrical 
tab but to have a consistent, reproducible process find a flux material 
suited for the task and a appropriate cleaning process.

Dave



"Glidden, Kevin" <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
09/21/2010 08:38 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Glidden, Kevin" <[log in to unmask]>


To
[log in to unmask]
cc

Subject
Re: [TN] Solderability of nickel plating






OK, pardon the lack of knowledge, but why is that?  I also see reference 
to nickel-boron platings, which supposedly improve both conductivity and 
solderability for electronics applications.

Is it recommended then that I need to apply gold over the EN on this 
electrical tab?  A portion of it is soldered (internally) and a portion of 
it remains exposed for connection (think 120V plug tabs).  The base 
material is brass.

Kevin Glidden
Manufacturing Engineer
Astronics Luminescent Systems Inc.

-----Original Message-----
From: vladimir Igoshev [mailto:[log in to unmask]] 
Sent: Tuesday, September 21, 2010 9:24 AM
To: TechNet E-Mail Forum; Glidden, Kevin
Subject: Re: [TN] Solderability of nickel plating

Kevin,

You wouldn't want to solder directly to unprotected  E-Ni.
Vladimir

SENTEC Testing Laboratory Inc.
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca

-----Original Message-----
From: "Glidden, Kevin" <[log in to unmask]>
Sender: TechNet <[log in to unmask]>
Date:         Tue, 21 Sep 2010 08:52:39 
To: <[log in to unmask]>
Reply-To: TechNet E-Mail Forum <[log in to unmask]>,
        "Glidden, Kevin" <[log in to unmask]>
Subject: [TN] Solderability of nickel plating

All,

Can anyone comment on the solderability of the nickel plate, particularly 
with regard to type of plating: high phosphor / low phosphor, and also 
storage conditions:

I've been gathering info, and seen conflicting information.

From one article: 
http://corrosion-doctors.org/MetalCoatings/Electroless.htm

A paper submitted at the Electroless Nickel conference of 1989 held in 
Cincinnati Ohio, Titled "Solderability Parameters of Elecroless Nickel 
Bearing Electronic Finishes" By Louis Kosarek of STB Systems, Inc. report 
that "An electroless nickel deposit which contains a concentration of 
phosphorus ranging from 0.1% to 3.0% is readily solderable on an 
"As-plated Basis" per Mil-Std 883c method 2003. The frequency of 
solderability tests which fail per Mil-Std 883c will increase as the 
phosphorus content of electroless nickel alloy increases from 3.0 to 7.0% 
phosphorus. A solderability test conducted per Mil-Std 883c method 2003 
incorporating an as-plated surface finish containing phosphorus in excess 
of 7%, the components will consistently fail. The mode of failure is 
non-wetting of the surface."
This indicates low phosphorous plating is best for solderability.  Many 
other papers seem to agree with this.

---------------------------------------------------------------------------------------------------------------------

From another article: http://www.pfonline.com/articles/pfd0024.html

Solderability/Weldability.  An important aspect of electroless nickel to 
the electronics industry is its solderability. All electroless nickel 
deposits are solderable provided the soldering conditions are matched to 
the condition of the particular electroless nickel deposit. 
Lower-phosphorus electroless nickel is more easily solderable immediately 
after plating than higher-phosphorus electroless nickel. However, this 
advantage disappears after 12 - 24 hrs. At this point, the ease of 
solderability depends upon the characteristics of the passive layer that 
forms on the surface of the electroless nickel deposit. Those deposits 
plated from baths containing heavy metal and sulfur-bearing brighteners 
and stabilizers, such as most commercial low- and mid-phosphorus 
electroless nickel systems, form a thicker tenacious passive layer than 
those that do not, such as most high-phosphorus electroless nickel 
systems. High-phosphorus electroless nickel systems tend to be more 
solderable in aged deposits.

Other important factors influencing the solderability of electroless 
nickel deposits include residual contamination left on the surface after 
plating and storage conditions after drying. Surface contamination and 
exposure to environments containing sulfur dioxide, chlorine, high 
humidity and high ambient temperatures will detrimentally affect 
solderability. Therefore, it is imperative that parts be thoroughly rinsed 
in clean DI water, dried and stored in a cool, dry atmosphere, preferably 
nitrogen.
This article indicates high phosphorous plating is best for long term 
solderability, and also that parts must be stored carefully (cool, dry, 
sealed, nitrogen).  Other articles seem to state this is a highly stable 
finish and is even used as a corrosion inhibitor.

Thanks,


Kevin Glidden
Manufacturing Engineer
Astronics Luminescent Systems Inc.<http://www.astronics.com>
4 Lucent Drive
Lebanon, NH 03766
(603) 643-7766 x3152

Please note, LSI operates on a 9/80 work schedule, and is closed on 
alternating Fridays.  Please click the link provided to view the days LSI 
will be closed.
http://www.astronics.com/LSI/documents/2010calendar-NH.pdf

NOTICE: This communication is intended specifically for the recipient(s) 
named above and may include proprietary, confidential or privileged 
information. If you are not a named recipient, you should immediately 
delete or destroy all electronic and physical copies of this 
communication. Unintended recipients also should not utilize, repeat, 
publish or relay to any other person the information contained herein nor 
should they take any action based upon, in whole or in part, such 
information. If you have received this message in error, you are requested 
to contact the sender immediately.

EXPORT COMPLIANCE STATEMENT: The information contained herein is or may be 
controlled by the International Traffic in Arms Regulations (ITAR), 22 CFR 
120-130, or the Export Administration Regulations (EAR) and may not be 
exported, or disclosed to a foreign person, whether in the United States 
or abroad, without prior U.S. Government and Astronics Luminescent Systems 
written approval. Violations of these regulations could result in 
administrative, civil or criminal penalties.  If you have any questions 
about the nature of the material contained in this email please contact 
the sender immediately.


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------



______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2