Hi gang - Chris, one thing you need to get more data on - the exact
component finish. As Gaby and Steve mentioned, if the component had a
bright acid tin finish, what you could be seeing is the codeposited
organics showing their presence during soldering. But - as Steve described
- TI components typically have a Ni/Pd/Au surface finish. If that is the
case, then the issue could possibly be insufficient soldering temperature.
The solder on the pads and the component surface finish haven't coalesced
which sometimes points to too low a soldering temperature or incorrect
reflow profile.
Dave Hillman
Rockwell Collins
[log in to unmask]
Gabriela <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
08/06/2010 01:16 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Gabriela <[log in to unmask]>
To
[log in to unmask]
cc
Subject
Re: [TN] blumpy
Yes, Dave is right. I had them too and had fun popping the big ones.
See that the leads which are at the ends of the part-look like mounting
spacers- don't have this defect because they are from a different batch of
leads and are OK.
There is a big chance that leads with this defect would have been OK for
through hole mounting and would have passed without detection of the
plating
with excess of organic brighteners .
Gaby
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: е 06 аевеси 2010 20:54
To: [log in to unmask]
Subject: Re: [TN] blumpy
Hi Chris!
Looks just like what I had back in Tulsa. I started calling what I saw
"Blumpy" (bumpy + lumpy = blumpy) ;^)
http://stevezeva.homestead.com/files/Connector_Blumpies.jpg
Dave Hillman and a few others said that it was co-deposited organics from
bright tin plating.
To me, the solder joints in the picture look like "head-in-pillow" joints.
I
wouldn't accept them and I would reject the parts back to the vendor. The
part looks like a TI part. I thought TI was plating their leads with
palladium and not tin though...
Steve
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Chris Mahanna
Sent: Friday, August 06, 2010 1:35 PM
To: [log in to unmask]
Subject: [TN] blumpy
So a customer has the blumpies (see link to pictures below). The hand
(dry)
solder melt-front smokes like a freight train under the microscope.
My questions are:
Have we really coined "blumpy"? and
If it wets and forms proper fillets, is it conformant?
Thanks!
Chris
This message contains attachments delivered via ShareFile.
- 30910 as soldered.jpg
- 30910 heel as recvd.jpg
Download the attachments here -
https://robisan.sharefile.com/d-TEMP-80276654fa1bea874e093013e1b
-----------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
__________ Information from ESET NOD32 Antivirus, version of virus
signature
database 5347 (20100806) __________
The message was checked by ESET NOD32 Antivirus.
http://www.eset.com
__________ Information from ESET NOD32 Antivirus, version of virus
signature
database 5347 (20100806) __________
The message was checked by ESET NOD32 Antivirus.
http://www.eset.com
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|
|
|