TECHNET Archives

August 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Torsten Hagge <[log in to unmask]>
Date:
Thu, 26 Aug 2010 18:38:50 +0200
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Inge <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
8bit
Content-Type:
text/plain; format=flowed; charset="iso-8859-1"; reply-type=original
From:
Parts/Attachments:
text/plain (180 lines)
We do no rely on soldered battery connection on boards. One antique but good 
solution is to crimp an eyelet on the cable and then use a screw or 
screw/nut/locking washer arrangement. You can run lots of current through 
such a connection without getting local heating and or milliohm problems. 
This kind of battery cable connection does not degrade with time like a 
direct solderd wire. Another one is to crimp a sleeve on the strands and 
then solder the assembly in feedthrough holes on the board. There are many 
more solutions.


/Inge


----- Original Message ----- 
From: "Torsten Hagge" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Thursday, August 26, 2010 5:46 PM
Subject: [TN] AW: [TN] soldered battery wire - breaking problem


Hi Carl,

as this process is not save for automotive we have to use special plastic 
strain reliefs where presoldered cables are placed in the plastic. Advantage 
is a faster assembly time and a safe process at our line.
Vendor e.g. is www.provertha.com, technology is called "wire clip connection 
technology".
best regards,
torsten

Dipl.Ing.(FH)Torsten Hagge
tech. projectmanager
Kristronics GmbH
Gewerbegrund 5 - 9
24955 Harrislee

Tel.:    +49 461 7741 624
Fax:     +49 461 7741 642
[log in to unmask]
www.kristronics.de

Gerichtsstand Flensburg, Handelsregister: HRB 1433 FL
Geschäftsführer Dipl.-Ing. oec. Thormod Ohm
Ust-Id-Nr. DE 811182059
Bankverbindung: Deutsche Bank AG Flensburg, Konto-Nr. 4216610, BLZ 21570011
IBAN: DE32 2157 0011 0421 6610 00, BIC: DEUT DE HH 215

-----Ursprüngliche Nachricht-----
Von: TechNet [mailto:[log in to unmask]] Im Auftrag von Carl VanWormer
Gesendet: Donnerstag, 26. August 2010 16:37
An: [log in to unmask]
Betreff: [TN] soldered battery wire - breaking problem

We produce a small module that is powered by a small battery in a
plastic battery holder that has the standard red & black wires, which
solder into two holes in in our PC board.  After initial functional
testing, the board (with battery holder attached) is sent out for
conformal coating, then the boards are re-tested before inserting into
our plastic enclosure.  The most recent run of 50 boards returned from
conformal coating with about 10 broken wires, with the break leaving
Copper colored ends visible where the strands were ripped from the
solder filled mounting hole.  Since this problem is new, something in
the assembly process (or conformal coating process) must have changed.
Once the battery holder and board are assembled into the plastic case,
there is no more strain on the wires, so this is only a production and
handling problem.



In reviewing the recent wire solder joints, compared to 2 samples from
previous runs that did not exhibit this problem, I noticed that the
"bad" assemblies had been heated enough to flow solder up into the wire
strands, while the "good" assemblies had solder on the wire ends on the
back side of the board, but the solder did not flow up the strands on
the front side of the board.  I'm guessing that the fused wire strands
are stiffer, and this is the cause of the breakage during handling for
the conformal coating process.



Many of us "old timers" remember the classic strain relief approach used
in the battery wires for transistor radios, where the two wires were
laced through a strain relief hole before being soldered onto the board.
Since our board has no room for the extra strain relief holes, and since
we have made hundreds of these things without problems, I'm looking for
suggestions on the best approach to solder the wires onto the board to
help eliminate the problem.



Are there any IPC standards for attaching battery holder wires?



Thanks,
Carl





Carl Van Wormer, P.E., AE7GD

Senior Hardware Engineer

Cipher Systems

1800 NW 169th Place, Suite B-100

Beaverton, OR  97006

Cipher Systems (503) 617-7447 x 5163

Direct Line (503) 425-5163

[log in to unmask] <mailto:[log in to unmask]>

This message may contain confidential and/or proprietary information,
and is intended for the person/entity to whom it was originally
addressed. Any use by others is strictly prohibited.  If I sent this to
you by mistake, please be nice and delete it, then tell me of my mistake
so I can send it to the right person.




______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
----------------------------------------------------- 


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2