We assemble limited quantities of polyimide rigid-flex assemblies. Due to moisture absorption by the polyimide substrate, we perform a bake prior to mass soldering processes; either reflow, wave or single point selective soldering.
We have recently found some vias near hand soldered locations on the rigid portion of the substrate that are open. Cross sections reveal the opens are at the interface between the rigid substrate and the flexible substrate. We have not specified a bake prior to hand soldering components on the rigid portion of the rigid-flex assembly. We are using Sn63Pb37 solder.
Is the open caused by TCE differences between the rigid and flexible substrates or by moisture turning to steam?
Is it necessary to bake polyimide rigid-flex substrates prior to hand soldering?
Is this inherent in all polyimide rigid-flex substrates or do we have a weakly bonded substrate?
Dick Krug, CSMTPE
SMT Process Engineer
Sparton Corporation
30167 Power Line Road
Brooksville, FL 34602-8299
p (352) 540-4012 (Internal Ext. 2012)
[log in to unmask]
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|