Hi Wayne,
...but there are. all you have to do is look at IPC-D-279 for guidelines. There cannot be requirements, because everybody's details/needs are different.
Werner
-----Original Message-----
From: Thayer, Wayne - IIW <[log in to unmask]>
To: [log in to unmask]
Sent: Wed, Jul 21, 2010 9:18 am
Subject: Re: [TN] solder joint height
Hi Werner-
You may recall I brought this issue up a few months ago too. The basic question
I have is
If solder joint height is important for longevity/reliability, why aren't there
IPC guidelines/requirements for them? As noted previously, tungsten rods are
available in almost any diameter and they can be used as a simple "quick check"
tool for this application.
Wayne
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier
Sent: Tuesday, July 20, 2010 1:01 PM
To: [log in to unmask]
Subject: Re: [TN] solder joint height
)Dale,
The answer is a qualified YES.
What are the sizes of these ceramic chip components and the Alloy-42-dominated
SOT? When do you see those cracks [thermal history]? What are the QUAL
requirements?
What is the real use environment?
I take it this is SnPb solder.
Regardless of these answers, a greater SJ height enhances reliability-you may
want to take a look at the attached reliability article (Engelmaier,W.,
"Achieving Solder Joint Reliability in a Lead-Free World, Part 1," GlobalSMT &
Packaging, Vol. 7, No. 6, June 2007, pp. 40-42). .
Werner
-----Original Message-----
From: Hart, Dale L CTR USAF AFMC AFRL/RXSA <[log in to unmask]>
To: [log in to unmask]
Sent: Tue, Jul 20, 2010 12:51 pm
Subject: Re: [TN] solder joint height
Air Force often uses CCA's as circuit card assemblies, sorry for the confusion.
The type of components are surface mount resistors, capacitor and I believe a
SOT with gull wing leads.
My problem is do I suggest their solder joint height isn't sufficient enough to
ensure a reliable assembly on an aircraft.
dlh
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier
Sent: Tuesday, July 20, 2010 11:19 AM
To: [log in to unmask]
Subject: Re: [TN] solder joint height
Hi Dale,
Do you mean CGA's [column grid arrays]? If not, what do you mean by cca?
610, Class 3 or otherwise, only addresses quality, not reliability-for that you
need to go to IPC-D-279.
While the absence of solder fillets can reduce fatigue life, the presence of
fillets, 'robust' or otherwise, does not have any positive first-order impact.
However, solder joint height does.
You may be looking at IMC crystals.
Werner
-----Original Message-----
From: Hart, Dale L CTR USAF AFMC AFRL/RXSA <[log in to unmask]>
To: [log in to unmask]
Sent: Tue, Jul 20, 2010 9:23 am
Subject: [TN] solder joint height
We have been doing a some analysis of cca's for the Air Force consisting of
SMT. The visual inspection of the solder joints looks very good all
characteristics above the suggest minimum for class 3 of 610. The solder
fillets in some instances could be characterized as being robust. In
cross-sectional analysis however, the solder joint height of the components
electrical termination above the land has been perhaps 0.025 mm to the point
of needing a SEM to look at the land-solder-component lead interface.
Closer examination in these areas revealed small cracks in the grain
boundaries. I used the term grain boundaries because the solder in these
areas do not resemble the colonies observed in the bulk solder of the
fillet. In some of these instances the land is often deformed in the shape
of the component lead.
Would these joints although stronger be more susceptible to fatigue or
overload failure?
What are the implications if these cca's are encapsulated?
What suggestions could be offered to the manufacturer?
Dale L. Hart
Universal Technology Corporation (UTC)
Failure Analysis
1270 North Fairfield Road
Dayton, Ohio 45432-2600
(937) 656-9165
Fax (937) 656-4600
Email: <mailto:[log in to unmask]> [log in to unmask]
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
This e-mail and any files transmitted with it may be proprietary and are
intended solely for the use of the individual or entity to whom they are
addressed. If you have received this e-mail in error please notify the sender.
Please note that any views or opinions presented in this e-mail are solely those
of the author and do not necessarily represent those of ITT Corporation. The
recipient should check this e-mail and any attachments for the presence of
viruses. ITT accepts no liability for any damage caused by any virus transmitted
by this e-mail.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|