Hi Kevin - there is a reasonable body of data documenting the use of the
Sn62 solder alloy for minimizing the leaching of silver into a solder
joint during solder processing. The effect is not large but has been used
widely throughout the industry. The addition of the 2%Ag content to the
Sn62 tin/lead alloys slows down but does not stop the dissolution of
silver from the item you are soldering. The AWS Soldering Handbook (ISBN
0-87171-618-6) has some information and a google search should yield some
published papers. The topic of silver acting as a solder joint reliability
improvement constituent for SnPb alloys is a much more controversial
topic. As Werner detailed, silver as been shown to strengthen solder
properties but how/if that characteristic improvement results in a
practical improvement of the solder joint is still a lively discussion.
The majority of the industry has utilized the Sn62 for its
leaching/wetting characteristics (i.e. tombstoning of small SMT chip
components) rather than for a solder joint reliability reason.
Dave Hillman
Rockwell Collins
[log in to unmask]
"Glidden, Kevin" <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
07/14/2010 12:24 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Glidden, Kevin" <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] silver solders and thermal fatigue resistance
Greetings,
Can anyone provide a simple description of or provide/recommend articles
regarding the role of silver addition in solders? I've seen reference in
several articles that it was originally used as a means to mitigate
migration of silver when soldering to thick silver deposits. I've also
seen reference that it also increases the thermal fatigue resistance. The
latter is what I am most interested in, and would like to better
understand the "why's".
Thanks,
Kevin Glidden
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|