Inge,
Typical SAC305 solder paste. We are fully RoHS compliant.
Bev
RIM
-----Original Message-----
From: Inge [mailto:[log in to unmask]]
Sent: Friday, June 11, 2010 11:50 AM
To: Bev Christian; [log in to unmask]
Subject: Re: [TN] Weird formation of voids
Does the solder paste have Silver adds?
Inge
--------------------------------------------------
From: "Bev Christian" <[log in to unmask]>
Sent: den 11 June 2010 17:40
To: <[log in to unmask]>
Subject: Re: [TN] Weird formation of voids
> Stewart,
> I lieu of a Dave Hillman Friday quiz, consider this it. And you WIN!
> Using an SEM and then carefully examining those pictures and the shape and
> placement of the "voids" we were able to determine that it is exactly as
> you describe. We are now in the process of hitting our grinding paper
> supplier "up the side of the head" for a crappy lot of product.
>
> Bev
> RIM
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Stewart McCracken
> Sent: Friday, June 11, 2010 11:36 AM
> To: [log in to unmask]
> Subject: Re: [TN] Weird formation of voids
> Importance: High
>
> Hi All,
>
> Looks as though sample preparation condition is less than ideal. Sample is
> a little rounded and it appears that the voids might in fact be embedded
> debris from the polishing equipment(?) I'm sure Vladimir would agree - get
> it in the SEM to be sure! Need some better imaging and if possible EDS -
> these will go a very long way to confirming what's going on. Lumps of
> silicon carbide can really make a mess of a x-section. If you don't have
> access to a SEM, you could etch the structure and look for abnormal
> /unusual structures surrounding these features. Etching would also help to
> refine the soft edges on a x-section (provide a more natural edge) and let
> you see if you have shrinkage or gas voids (look at shape) filled with
> grinding debris.
>
> Contaminated mats on a polishing station could explain the pattern of
> occurrence and the feature. As always though, more info about condition
> would make diagnosis easier!
>
> Kind regards,
>
> Stewart
>
> Stewart McCracken
> MCS Ltd.
> Centre House
> Midlothian Innovation Centre
> Roslin
> Midlothian
> EH25 9RE
>
> m. +44(0)7711 541735
> t. +44(0)131 440 9090
> f. +44(0)131 440 9085
> e. [log in to unmask]
> w. www.themcsgroup.co.uk
>
>
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of stephen gregory
> Sent: 11 June 2010 16:21
> To: [log in to unmask]
> Subject: Re: [TN] Weird formation of voids
>
> Hi Bev!
>
> Got your picture today, and have it posted now:
>
> http://stevezeva.homestead.com/Bevs_Ball.jpg
>
> Almost looks like little pieces of dross. I wonder if something is going
> on with the solder paste? Or leaded reflow profile with a lead-free BGA?
>
> Steve
>
> --- On Wed, 6/9/10, Bev Christian <[log in to unmask]> wrote:
>
>
> From: Bev Christian <[log in to unmask]>
> Subject: [TN] Weird formation of voids
> To: [log in to unmask]
> Date: Wednesday, June 9, 2010, 9:51 AM
>
>
> TechNetters,
> I am sending a picture to Steve to post. I have labs in three locations.
> One of them has seen weird voids in cross-sections of BGAs while the other
> two locations have not. For the lab that has seen them, the
> cross-sections were prepared by different people on different days for
> different products, using the same equipment. The voids are not in all
> balls cross-sectioned but may be only in one of two of the balls in a row
> of multiple solder joints examined.
>
> Have you seen anything like this? Do you know the root cause?
>
> Vlad,
> You know what is going on, so please don't respond.
>
> Bev
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
>
> ---------------------------------------------------------------------
> This transmission (including any attachments) may contain confidential
> information, privileged material (including material protected by the
> solicitor-client or other applicable privileges), or constitute non-public
> information. Any use of this information by anyone other than the intended
> recipient is prohibited. If you have received this transmission in error,
> please immediately reply to the sender and delete this information from
> your system. Use, dissemination, distribution, or reproduction of this
> transmission by unintended recipients is not authorized and may be
> unlawful.
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|