I vote with Ian and Groovy Hoovy.
This is a classic void. The copper edge is convex suggesting copper was depositing at the edge of an un-plate-able area. There was either no electroless or some resist where the void occurred.
Since it is technically a "ring void" (thank you Chuck) I expect that there may have been a ring of resist residue from developing or a contaminated rinse. But if it is a 360° ring void how did it pass electrical test? I would call it a "half moon" void but that would be lunie.
It is not an etching void because if this were an etch-out the edge would be concave.
It could not be a bubble because how could a bubble be so flat. It can't be two bubbles because small bubbles would rise to one side of the hole.
Sincerely,
Paul Reid
Program Coordinator
PWB Interconnect Solutions Inc.
235 Stafford Rd., West, Unit 103
Nepean, Ontario
Canada, K2H 9C1
613 596 4244 ext. 229
Skype paul_reid_pwb
[log in to unmask] <mailto:[log in to unmask]>
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Al Onderick
Sent: June 17, 2010 5:04 PM
To: [log in to unmask]
Subject: [TN] Thursday Quiz
What causes this ?
http://www.austinwoodsandwaters.com/open-via.jpg
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|