Yes, and I found it was trapped volatile material between the lead plating and the lead base material...
Try baking the QFP to a bone dry condition per the manufacturer spec then assemble the PCA...
Paul
Paul Edwards
Surface Art Engineering
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Guy Ramsey
Sent: Monday, June 28, 2010 5:01 AM
To: [log in to unmask]
Subject: Re: [TN] QFP short at top of the leads - Found word(s) list error in the Text body
http://www.uyemura.com/solder_joint_reliability.htm#5
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M.
Sent: Monday, June 28, 2010 7:34 AM
To: [log in to unmask]
Subject: Re: [TN] QFP short at top of the leads
Wayne,
What makes ENEPIG incompatible with SnPb solder?
Regards,
George
George M. Wenger
Andrew Solutions
Senior Principal FMA/Reliability Engineer
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 (Office) (732) 309-8964 (cell)
[log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Thayer, Wayne - IIW
Sent: Monday, June 28, 2010 7:21 AM
To: [log in to unmask]
Subject: Re: [TN] QFP short at top of the leads
Need to know the metallurgy. What is the lead plating spec, and what alloy
are you soldering with? Note that ENEPIG is incompatible with SnPb solder.
Wayne Thayer
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Rex Waygood
Sent: Monday, June 28, 2010 6:53 AM
To: [log in to unmask]
Subject: Re: [TN] QFP short at top of the leads
Are these virgin parts?
Are the leg to pad joints 'good'?
Rex
Rex Waygood
Technical Manager
Hansatech EMS provides value manufacturing through engineering and
quality
Hansatech EMS Limited
Benson Road
Nuffield Industrial Estate
Poole
Dorset
BH17 0RY
+44 (0)1202 338200
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Iven, Jowan
Sent: 28 June 2010 10:08
To: [log in to unmask]
Subject: [TN] QFP short at top of the leads
Has anyone ever seen a QFP where shorts occur after soldering at the top
of the leads?
And the leads look pretty dull after soldering. Any ideas?
A picture is available at
http://ipc-technet.groupsite.com/uploads/galleries/x/000/020/5ba/technet
01.jpg
Jowan Iven
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
This e-mail and any files transmitted with it may be proprietary and are
intended solely for the use of the individual or entity to whom they are
addressed. If you have received this e-mail in error please notify the
sender.
Please note that any views or opinions presented in this e-mail are solely
those of the author and do not necessarily represent those of ITT
Corporation. The recipient should check this e-mail and any attachments for
the presence of viruses. ITT accepts no liability for any damage caused by
any virus transmitted by this e-mail.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
==============================================================================
This email and any attachments thereto may contain private, confidential, and
privileged material for the sole use of the intended recipient. Any review, copying,
or distribution of this email (or any attachments thereto) by others is strictly prohibited.
If you are not the intended recipient, please contact [log in to unmask]
immediately and permanently delete the original and any copies of this email and
any attachments thereto.
==============================================================================
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|