Inge,
Agree on toe fillets - or absence thereof.
For side fillets, if none there or one missing, I would x-section to check for good intermetallic between the bottom of the lead and the solder. If it is there, I would not see a problem.
UK NPL says at most toe fillets could provide 5% of the joint strength and side fillets 20%. Most of the strength is in the heel fillets.
Bev
----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Tue May 18 16:44:55 2010
Subject: Re: [TN] Acceptabe Solder Fillet on Gull wings
Hi Robert,
strange name on your company, how do you pronounce it?
To start with, I have pretty much litterature on soldering, but after so
many years confronting soldering, I seldom need look in the book shelf.
However, I did in your case. Wassink has a whole chapter about solder
failures, and in special what he calls ' Soldering Defects Fault Finder
Diagram' Lots of defects are mentioned but not a word about side fillets.
Moreover, most gurus claim, that what is alpha and omega is the solder
fillet between the lead's underside and the solder pad of the board. The
wetting on the sides of the leg, the side fillets, do not play a significant
role according to some authors. Well, that may be so, and the IPC got its
requirements as you mention. Myself, I allow myself to have a quite
different opinion. I've participated in control and inspection documents for
Ericsson for many years, and the operators follow my instructions
meticulously. I mean, that solder fillet on one side only can't be
acceptable for a high quality production process. It has not to do with any
mechanical aspect nor any strength or fatigue calculations. It has simply to
do with the quality of the general lead finish. If there is a one side ony
fillet, we immediately suspect that there may be a plating problem or a
wetting issue. And we never take the risk of accepting such solder joints.
On the 'toe' question, I say it depends on whether the leg is plated befor
or after leg cutting. If the legs are cut after the plating, you cannot
demand solder wettin of course.
The TN gurus will probably do protest, but in this case, I will not take
one step backwards.
Inge
--------------------------------------------------
From: "Robert N" <[log in to unmask]>
Sent: den 18 May 2010 21:07
To: <[log in to unmask]>
Subject: [TN] Acceptabe Solder Fillet on Gull wings
> IPC 610 Cl 2 states that a side overhang of 50% is acceptable. Does that
> means, which seems obvious but not stated, that an acceptable solder
> fillet is
> required on one side only? Does the same apply to the toe, which allows
> for
> an overhang?
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-615-7100 ext.2815
> -----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|