Wayne,
Ferric Chloride is of the 70's last century. The etch speed is
decreasing with increasing copper content. The ferrous in the
solution cannot be replenished into ferric, the cuprous not easily
separated/extracted from the depleted etchant. After etching the
boards, much of rinse water is required due to the viscosity of the
etchant. And how do you get rid of the exausted etchant? Do you have a
buyer for this? Dumping in the environment has to be avoided (often
did by hobby PCB-makers).
In the past I used acidous cupric cloride with hydrogen peroxide and
hydro chloric acid as replenishment liquids. Advantage is that you can
see when replenishment is required (darkening of the light green fresh
etchant). Hydrogen peroxide and hydro chloric acid is easily available
at the drug store, resulting in an increasing amount of etchant. The
surplus etchant can be easily sold for its clean copper content.
In the solution you have to control the copper content on about 30
w/w%. Acidity pH= ~ 1.0.
Copper etchants can more easily rinsed than ferric etchants.
Regards,
Peer Langeveld
Consultant Soft Soldering Processes
5502 VH 8 The Netherlands
2010/5/13 Thayer, Wayne - IIW <[log in to unmask]>:
> MG chemicals sells pre-sensitized circuit board material. Artwork can be generated by transparency on laser printers, but you usually get better results with ink jets. You can also use the "toner transfer" technique on non-pre-sensitized laminate (google that and you should get some nice pix). Resolution will be limited to approximately 10mil line and space.
>
> Aligning one side of the artwork with the other can be challenging too. You'd like to drill the holes first so you can align the artwork to the holes, but then you can't use pre-sensitized material. When I used boards made this way, I etched a tiny hole in each of the vias which gave me a visual drill target for use on a small drill press(like a dremel tool drill press).
>
> Ferric Chloride is the preferred etchant for hobbyist use. Stains everything in the area!
>
> Forget about plated vias. You can use eyelets. Hand setting them is a pain, though, and you should solder them in anyway for the best performance, so replacing them with a small piece of wire works too, and can be done on tighter geometries. You can get away with almost anything for soldermask. I've used spraycans of Rustoleum.
>
> Don't bother with "liquid tin". It makes the results look a bit nicer, but the consensus is that it doesn't solder significantly better than corroded copper.
>
> The results will be very crude but useable. Note that getting a simple board like this done at a pcb house set up for prototypes will only be a couple of hundred dollars and about 2 days, so if your time is worth much you won't be saving anything by rolling your own!
>
> Wayne Thayer
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Toby Carrier
> Sent: Thursday, May 13, 2010 1:06 PM
> To: [log in to unmask]
> Subject: [TN] Hobbyist PCB Fab Equipment
>
> Hello all,
>
> I want to start making PCB's at home for prototyping small to medium
> projects, but I have a few questions about materials, kits and equipment:
>
> 1. What is the best kit to buy?
> 2. What equipment do I need?
> 3. Where is the best place to get the equipment and/or kits?
> 4. What safety hazards do I need to worry about?
>
> I will be dealing with through-hole and surface mount parts.
>
> Thanks for the help.
>
> Toby Carrier
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
> This e-mail and any files transmitted with it may be proprietary and are intended solely for the use of the individual or entity to whom they are addressed. If you have received this e-mail in error please notify the sender.
> Please note that any views or opinions presented in this e-mail are solely those of the author and do not necessarily represent those of ITT Corporation. The recipient should check this e-mail and any attachments for the presence of viruses. ITT accepts no liability for any damage caused by any virus transmitted by this e-mail.
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|