Steve,
Awesome. Now that you've walked me through it, I think our customer has a mixed bag- some bond lifts and delam, all damaged by excessive soldering excursions. I guess maybe part of my question was whether delam was a latent defect from poor bonding.? Haven't found significantly necked down Au wires yet.
Do you think they can get significantly better CTE, Tg out of blue lenses? On our job, the blue had half the failure rate of the clear, even though they are rated the same for soldering. BTW they are both really Ir emitters; clear lenses with the better spectrum.
Thanks for the help. I will certainly try to get permission to post the pictures. I'd like to see Vladimir's SEM image. Is there further FA to be gleaned from SEM?
Thanks Werner!
Wayne, yes I believe that was the official blame game from the component manufacturer. What do they look like when you burn them up? I'd expect to see burnt plastic too.??
Chris
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steven Creswick
Sent: Monday, May 10, 2010 6:49 PM
To: [log in to unmask]
Subject: Re: [TN] LED wiring bonding
Chris,
Ahh! Something I can help out with.
A great deal depends on the package structure, obviously wire bonding
process control, and whether it is Au or Al wire.
Wire bonding defects are rare, if the materials and process is under
control.
The caveat is that Pb-free reflow temps may cause extra expansion in the
molding compound as the material goes above it Tg during reflow/s.
Many/most clear mold compounds have Tg's in the <135-155°C range. Can't put
silica in there to help modify the CTE...
Moving mold compound during temp cycles can often break the bond wire near
mid-span. The wire will actually neck down to the shape of an hour-glass
funnel as it stretches. ... then breaks. Oops.
You can also get bond lifts, but if that is the case you may also see
delamination from the bonding surface. Hard to describe what it looks like
other than to say that you can see an air-gap there.. If you don't see the
delam, one just may have a poor bond.
You can also shear the ball/bond off the die, but many times one will place
a low modulus material on top of the chip to mechanically de-couple from the
higher modulus molding compound in an attempt to alleviate this.
First thing to do is x-ray to find where the discontinuity is. If that
fails, then move on to selectively polishing the device down so that you can
see inside clearly.
I have been known to take a really tiny 0.010-0.015" dia drill bit in a pin
vise to gain access to the interior for dye testing to check for
delamination [but that can be classified as destructive - although certainly
illustrative!]
Lastly, it may also be possible to shear the die off, but like you, I would
look at the wire first. A quick look at the bonds can often tell you if
they are over bonded, or something was moving during bonding. Once you get
it polished flat, you may be able to get a reasonable picture.
Steve Creswick
http://www.linkedin.com/in/stevencreswick
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Chris Mahanna
Sent: Monday, May 10, 2010 5:49 PM
To: [log in to unmask]
Subject: [TN] LED wiring bonding
It's all LEDs these days!
We have an FA that shows poor wire bonds to GaAlAs/GaAs in microsection
after assembly. The failure is seen in the parts per hundred across
different lots and slightly different part numbers of LEDs.
The assumption would be that LED wiring bonding defects are very rare. Is
there something particular about these? Or is it the crimping and/or
Pb-free assembly that is pulling them apart?
The ones that seem more susceptible are GaAlAs Double Heteros.
Thanks.
Chris
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|