TECHNET Archives

May 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Date:
Thu, 6 May 2010 08:15:04 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Ioan Tempea <[log in to unmask]>
Subject:
From:
Ioan Tempea <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (210 lines)
Doug,

I wish the substance was old... and smart, like us!

You are putting me in a tough situation here. How to check surface energy, what should be the good values and how to fix it if not OK?

Thanks,

Ioan Tempea, ing.
Ingénieur Principal de Fabrication / Senior Manufacturing Engineer
T | 450.967.7100 ext.244
E | [log in to unmask] 
W | www.digico.cc

N'imprimer que si nécessaire - Print only if you must


-----Message d'origine-----
De : Douglas Pauls [mailto:[log in to unmask]] 
Envoyé : May-06-10 8:10 AM
À : [log in to unmask]
Objet : Re: [TN] Wrinkling of conformal coating

For what it is worth, I think that the coating is simply too old. Isn't 
the cause for most wrinkles?  Some days I just slay me.

One thing that you might check as well is the surface energy of your 
masked surface.  Some of the other suggestions from the forum are your 
more likely culprits, but you may be seeing some form of dewetting as 
well, that causes the coating to pull away from one area and congregate in 
another.  Sometimes it is not the mask, but how the mask has been 
processed that is the issue.


Doug Pauls



Graham Collins <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
05/05/2010 02:13 PM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
[log in to unmask]


To
[log in to unmask]
cc

Subject
Re: [TN] Wrinkling of conformal coating






For my guess I'll go with either too thick, or contamination on the panel 
making it try to dewet.

Questions: is this a new problem on a product you have been successfully 
coating until now?  Have you measured the thickness to ensure it is within 
normal range?

Suggestion: Could you do two thinner coats and let it flash off a bit 
between coats?

regards, 
  
Graham Collins 
Halifax Production Engineering 
L-3 communications Electronic Systems 
(902) 873-2000 ext. 6215 

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan Tempea
Sent: Wednesday, May 05, 2010 3:59 PM
To: [log in to unmask]
Subject: [TN] Wrinkling of conformal coating

Dear Technos,

 

Back to orange peeling, this time concerning conformal coating, please see 
http://ipc-technet.groupsite.com/galleries/photo/124230

 

The coating is applied with an Asymtek Century machine and is a Conap 1170 
acrylic.

 

·         The board is left curing in ambient temperature, no 
acceleration. Starting with an even coating, in about 20-30 minutes the 
liquid seems to move towards a certain area (no rippling at this moment). 
After another 10-15 minutes the rippling effect sets in.

·         We thought that due to the almost 2 minutes lag between the 
coating of the first and last image, the drying of the coating layer is 
not even and the one side curing first pulls on the liquid at the other 
end. So we've cut the panel in 2, accelerated the machine, the problem is 
still there.

·         The boards are laid as flat as possible, maybe not perfectly 
horizontal, but not worse than others with the same coating, that do not 
show any issue

·         Just to make it more difficult: grabbed a non-populated panel 
from the stores, coated it, placed on the same flat surface, and guess 
what: no issues.

 

The PCB has Taiyo PSR 4000 MP soldermask.

 

So I would need your guidance in clarifying where is this coming from and 
how to fix it.

 

Thank you,

 

Ioan Tempea, ing.
Ingénieur Principal de Fabrication / Senior Manufacturing Engineer
T | 450.967.7100 ext.244
E | [log in to unmask] <mailto:[log in to unmask]> 
W | www.digico.cc <http://www.digico.cc/> 

 
 N'imprimer que si nécessaire - Print only if you must

 


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
for additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2