TECHNET Archives

April 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Date:
Tue, 27 Apr 2010 10:07:28 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Ioan Tempea <[log in to unmask]>
Subject:
From:
Ioan Tempea <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
<001601cae610$816fe660$844fb320$@com>
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (182 lines)
You know Steve,

I still have to figure out why the solder is that thin under the pins. Normal 6 mil stencil, good wetting around the pins, fair heel, as seen in the x-section. Pure Sn plating could have an influence on that, like solder going higher on the pin, wicking out from under?

Thanks,

Ioan Tempea, ing.
Ingénieur Principal de Fabrication / Senior Manufacturing Engineer
T | 450.967.7100 ext.244
E | [log in to unmask] 
W | www.digico.cc

N'imprimer que si nécessaire - Print only if you must


-----Message d'origine-----
De : Steve Gregory [mailto:[log in to unmask]] 
Envoyé : April-27-10 9:50 AM
À : 'TechNet E-Mail Forum'; Ioan Tempea
Objet : RE: [TN] Failure fatigue photos

Hi Ioan!

That lead style on that connector looks similar to the AMP connector that I
had the "blumpy" plating problem with remember?
They were a kind of stiff butt joint looking thing...

http://stevezeva.homestead.com/files/Connector_Blumpies.jpg

Mine was called a Densipac connector:

http://mouser.com/Search/include/LargeProductImage.aspx?path=tyco/lrg/inhous
e_913937549_t.jpg

I know your datasheet says they were tin/lead plated, but I bet you they
were pure tin.

I don't know if that has anything to do with anything....

Steve

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan Tempea
Sent: Tuesday, April 27, 2010 9:24 AM
To: [log in to unmask]
Subject: Re: [TN] Failure fatigue photos

Victor,

Zero rework, part is socket
http://www.tycoelectronics.com/catalog/pn/en/5-316365-0?RQPN=5-316365-0 ,
the IMC thickness has not been measured

And thank you Guenter, the lack of compliancy of this component has been
mentioned during design review. I'm so proud of myself...

Best regards,

Ioan Tempea, ing.
Ingénieur Principal de Fabrication / Senior Manufacturing Engineer
T | 450.967.7100 ext.244
E | [log in to unmask] 
W | www.digico.cc

N'imprimer que si nécessaire - Print only if you must

-----Message d'origine-----
De : Victor Hernandez [mailto:[log in to unmask]] 
Envoyé : April-27-10 9:12 AM
À : [log in to unmask]
Objet : Re: [TN] Failure fatigue photos

What type of component is this and what is the thickness of the IMC layer,
any associated rework on the device.

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan Tempea
Sent: Tuesday, April 27, 2010 8:00 AM
To: [log in to unmask]
Subject: [TN] Failure fatigue photos

Dear Technos,

It looks like, for the first time, I have the occasion to look at fatigue
failed joints. The lab analysis we've got states this, but does not abounds
in details.

One of the conclusions is "the crack propagates around harder Sn shearing
the softer Pb, but the Sn and Pb zones seem fairly large for regular solder
structure". Citing from Klein Wassink "During cyclic plastic deformation the
microstructure inside the material changes in the zones where the
deformation is concentrated. This leads to local grain growth..."

I have deposited the micro-sections on the IPCs website
http://ipc-technet.groupsite.com/gallery/13116

I would need your expert opinion regarding the failure. Is this fatigue? The
big pure Sn and pure Pb areas, are they normal size for fatigued joints?

Thanks,

Ioan Tempea, ing.
Ingénieur Principal de Fabrication / Senior Manufacturing Engineer
T | 450.967.7100 ext.244
E | [log in to unmask] <mailto:[log in to unmask]>  
W | www.digico.cc <http://www.digico.cc/> 
 
 N'imprimer que si nécessaire - Print only if you must

 ______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2