And on top of everything the size does matter in that particular situation.
Regards,
Vladimir
SENTEC Testing Laboratory Inc.
11 Canadian Road, Unit 7.
Scarborough, ON M1R 5G1
Tel: (416) 899-1882
Fax: (905) 882-8812
www.sentec.ca
-----Original Message-----
From: "David D. Hillman" <[log in to unmask]>
Date: Tue, 20 Apr 2010 11:06:42
To: <[log in to unmask]>
Subject: Re: [TN] SAC Shrinkage Voids in BGA Balls
Hi Werner - we are both on the same page (I should have typed out a more
detailed response). As you detailed, the actual metallurgical reactions of
shrinkage are the same, the focus should be on what is staying molten
last. We have observed on some BGA solderballs that were part of the
circuit connection to ground planes some slightly different shrinkage void
differences due to the solidification reactions. Interesting from a
technical viewpoint but didn't make a difference from a solder joint
integrity perspective.
Dave
Werner Engelmaier <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
04/20/2010 10:55 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Werner Engelmaier <[log in to unmask]>
To
[log in to unmask]
cc
Subject
Re: [TN] SAC Shrinkage Voids in BGA Balls
Hi Dave,
A shrinkage void in an ingot occurs where it solidifies last---in its
center.
The same is true for SJs, except that they do not necessarily cool from
the outside in. but a connected to various heatsinks and reservoirs---the
component is typically a heat sink [coolest] and the PCB is a reservoir
[hottest], with various heat transfer conditions on the surface due to
forced air/N2.
Overall, SJs tend to solidify first at their surface; hence, most
shrinkage voids are to be found there.
Werner
-----Original Message-----
From: David D. Hillman <[log in to unmask]>
To: [log in to unmask]
Sent: Tue, Apr 20, 2010 10:13 am
Subject: Re: [TN] SAC Shrinkage Voids in BGA Balls
Hi Bev - in theory, a shrinkage void in a solderball is the same physics
as a shrinkage void in a aluminum or steel casting so no, the shrinkage
void would not have to necessarily always reach a surface. However, after
looking at several hundred SAC BGA/CSP cross-sections, I have nearly
always (99.999%) found a path of a shrinkage void to the solderball
surface. Because we have a very limited and very small molten solder
"volume", I think you will find a surface connection. And I guess I'll
bite - why the question?
Dave Hillman
Rockwell Collins
[log in to unmask]
Bev Christian <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
04/20/2010 08:16 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
Bev Christian <[log in to unmask]>
To
[log in to unmask]
cc
Subject
[TN] SAC Shrinkage Voids in BGA Balls
TechNetters,
Do all SAC shrinkage voids in BGA balls reach/start at the surface of
the ball? I realize I may be stumped by a 2D cross-section of a 3D
phenomenon, but I thought I would ask this august body.
Bev
RIM
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute non-public
information. Any use of this information by anyone other than the intended
recipient is prohibited. If you have received this transmission in error,
please immediately reply to the sender and delete this information from
your system. Use, dissemination, distribution, or reproduction of this
transmission by unintended recipients is not authorized and may be
unlawful.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|