TECHNET Archives

April 2010

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Tue, 27 Apr 2010 17:19:26 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Steve Gregory <[log in to unmask]>
Subject:
From:
Steve Gregory <[log in to unmask]>
Content-Transfer-Encoding:
8bit
In-Reply-To:
<74DFBF76961E4089A22180D866788EB9@KontoretPC>
Content-Type:
text/plain; format=flowed; charset="iso-8859-1"; reply-type=response
MIME-Version:
1.0
Parts/Attachments:
text/plain (203 lines)
Hi Inge,

Here's your cross section photo:

http://stevezeva.homestead.com/VD0_8073_NEWXSECTION_6.jpg

I haven't tried posting a picture to the IPC photo library yet, don't really 
need to, I have my own page ;^>

Steve

--------------------------------------------------
From: "Inge" <[log in to unmask]>
Sent: Tuesday, April 27, 2010 4:22 PM
To: <[log in to unmask]>
Subject: Re: [TN] Failure fatigue photos

> Hi both of you,
>
> I made a job for Siemens once, about fatigue. The board behind the 
> instrument panel of a truck vibrated on the roads in South America, 
> resulting in lifted leads and the trucks became inoperable. I simulated 
> the situation in the vibrator lab, and could see clearly what happened. 
> Just as Dave told you, the crack will finally occur in a band which is 
> represented by fine structure on the one side and a coarse and elongated 
> on the other. It has partly to do  with the solidification to do, fine 
> grains closest to the legs and coarser the more you are from that site. 
> I'll send one very illustrative photo.  I've missed how to fix that 
> instantly. How do you bring the photos to that fast presentation URL?
>
> Inge
>
> --------------------------------------------------
> From: "David D. Hillman" <[log in to unmask]>
> Sent: den 27 April 2010 06:33
> To: <[log in to unmask]>
> Subject: Re: [TN] Failure fatigue photos
>
>> Hi Ioan - Do you have any optical photos of the fracture? Thermal cycle
>> fatigue failures typically develop "banding (aka microstructure
>> coarsening)" in the solder joint shear zone. The solder joint
>> microstructure evolves into distinct grains of tin and lead which shows 
>> up
>> better in optical photos. The fracture in your photos appears to be
>> fatigue but its hard to see the microstructure in your photos. I added a
>> photo of what typical  thermal cycle induced SnPb coarsening looks like 
>> on
>> the IPC Photo Gallery.
>>
>> http://ipc-technet.groupsite.com/gallery/13118
>>
>> Dave Hillman
>> Rockwell Collins
>> [log in to unmask]
>>
>>
>>
>> Ioan Tempea <[log in to unmask]>
>> Sent by: TechNet <[log in to unmask]>
>> 04/27/2010 07:59 AM
>> Please respond to
>> TechNet E-Mail Forum <[log in to unmask]>; Please respond to
>> Ioan Tempea <[log in to unmask]>
>>
>>
>> To
>> [log in to unmask]
>> cc
>>
>> Subject
>> [TN] Failure fatigue photos
>>
>>
>>
>>
>>
>>
>> Dear Technos,
>>
>>
>>
>> It looks like, for the first time, I have the occasion to look at fatigue
>> failed joints. The lab analysis we've got states this, but does not
>> abounds in details.
>>
>>
>>
>> One of the conclusions is "the crack propagates around harder Sn shearing
>> the softer Pb, but the Sn and Pb zones seem fairly large for regular
>> solder structure". Citing from Klein Wassink "During cyclic plastic
>> deformation the microstructure inside the material changes in the zones
>> where the deformation is concentrated. This leads to local grain
>> growth..."
>>
>>
>>
>> I have deposited the micro-sections on the IPCs website
>> http://ipc-technet.groupsite.com/gallery/13116
>>
>>
>>
>> I would need your expert opinion regarding the failure. Is this fatigue?
>> The big pure Sn and pure Pb areas, are they normal size for fatigued
>> joints?
>>
>>
>>
>> Thanks,
>>
>>
>>
>> Ioan Tempea, ing.
>> Ingénieur Principal de Fabrication / Senior Manufacturing Engineer
>> T | 450.967.7100 ext.244
>> E | [log in to unmask] <mailto:[log in to unmask]>
>> W | www.digico.cc <http://www.digico.cc/>
>>
>>
>> N'imprimer que si nécessaire - Print only if you must
>>
>>
>>
>>
>> ______________________________________________________________________
>> This email has been scanned by the MessageLabs Email Security System.
>> For more information please contact helpdesk at x2960 or [log in to unmask]
>> ______________________________________________________________________
>>
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 15.0
>> To unsubscribe, send a message to [log in to unmask] with following text in
>> the BODY (NOT the subject field): SIGNOFF Technet
>> To temporarily halt or (re-start) delivery of Technet send e-mail to
>> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>> To receive ONE mailing per day of all the posts: send e-mail to
>> [log in to unmask]: SET Technet Digest
>> Search the archives of previous posts at: 
>> http://listserv.ipc.org/archives
>> Please visit IPC web site 
>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>> for additional information, or contact Keach Sasamori at [log in to unmask] 
>> or
>> 847-615-7100 ext.2815
>> -----------------------------------------------------
>>
>>
>> ______________________________________________________________________
>> This email has been scanned by the MessageLabs Email Security System.
>> For more information please contact helpdesk at x2960 or [log in to unmask]
>> ______________________________________________________________________
>>
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 15.0
>> To unsubscribe, send a message to [log in to unmask] with following text in
>> the BODY (NOT the subject field): SIGNOFF Technet
>> To temporarily halt or (re-start) delivery of Technet send e-mail to 
>> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>> To receive ONE mailing per day of all the posts: send e-mail to 
>> [log in to unmask]: SET Technet Digest
>> Search the archives of previous posts at: 
>> http://listserv.ipc.org/archives
>> Please visit IPC web site 
>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional 
>> information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 
>> ext.2815
>> ----------------------------------------------------- 
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask] 
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to 
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to 
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
> for additional information, or contact Keach Sasamori at [log in to unmask] or 
> 847-615-7100 ext.2815
> -----------------------------------------------------  


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2